<?xml version="1.0" encoding="utf-8" ?>















<feed version="0.3" xmlns="http://purl.org/atom/ns#" xmlns:dc="http://purl.org/dc/elements/1.1/" xml:lang="zh_CN">
<title><![CDATA[朝阳产业]]></title>
<link rel="alternate" type="text/html" href="http://cybx1118.blog.bokee.net"/>
<modified>2008-07-05T18-45-45 GMT+08:00</modified>
<tagline type="text/html" mode="escaped"><![CDATA[新型建材－－耐碱玻璃纤维网格布，保温钉的专业制造商]]></tagline>
<generator url="http://www.bokee.net/" version="2.0">bokee.net</generator>
<copyright>Copyright (c) 2005,  cybx1118</copyright>


<entry>
<title>建筑人生 </title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1959294.html"/>
<issued>2008-07-05T18-45-45 GMT+08:00</issued> 
<created>2008-07-05T18-45-45 GMT+08:00</created>
<modified>2008-08-22T06-21-12Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1959294</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>Default Cloumn</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<table cellspacing="0" cellpadding="0" width="812" border="0" class="da">
    <tbody>
        <tr>
            <td height="24">&nbsp;</td>
            <td valign="top"><blockquote>
            <h3>建筑人生 </h3>
            </blockquote></td>
        </tr>
        <tr>
            <td valign="top" colspan="2" height="473">
            <table cellspacing="0" cellpadding="0" width="100%" border="0">
                <!--DWLayoutTable-->
                <tbody>
                    <tr>
                        <td class="ziti" valign="top" width="587" height="462"><blockquote>
                        <p><font size="2">&nbsp;&nbsp;&nbsp;&nbsp; 人们为了追求美好的生活，而去工作，选择一种职业为之而奋斗。建筑者们选择了建筑事业，他们的一生在和建筑打交道，那一件件精美的工程，虽是钢筋混凝土组成的，却凝聚了建筑者们永恒的智慧、汗水和心血；默默静立的建筑其实凝聚着工程师们的灵魂，它们是凝固的音乐篇章，是无言的颂歌。曾经,对工程师的概念充满了崇拜的敬意，总是惊叹这么复杂的庞大事物是如何造成的，而今我身处在建筑单位，才深切体会到建筑者的艰辛与伟大。<br />&nbsp;&nbsp;&nbsp;&nbsp;环境的恶劣是任何人都不愿承受的，可是建筑者们却以苦为乐，苦中作乐，他们以百折不挠，坚忍不拔的开拓精神，攻克了一个又一个堡垒，一个又一个工程项目成为餐桌上的蛋糕。危难时刻挺得住，关键时刻冲得上，以大胆的创新精神和不断超越自我的勇气，迈向一个又一个新台阶。以不断开拓的进取精神，将事业推向一个又一个至高点。不畏艰难，勇于开拓的象征，是他们血汗和智慧的结晶。业绩是拼搏出来的，成功是来之不易的，没有超常的付出，就不会有相应的回报。没有拼搏的人生是暗淡无色的，只有拼搏才会有精彩的人生，拼搏是生命的动力！<br />&nbsp;&nbsp;&nbsp;&nbsp;当青春的容颜呈现出衰老的痕迹时，那是用精美的工程作为报酬的，是为世代人造福的成果换去的。建筑者们自己掌握命运的舵盘，充分显示自我价值。任风雨在他们的容颜上侵蚀，任自己的生命释放在荒山僻岭，任自己的心灵孤寂地守候在一件件工程之中。<br />&nbsp;&nbsp;&nbsp;&nbsp;我知道,在他们的人生价值中，奋斗，是一种生生不息的生命力，生命不息，战斗不止，对困难的克服，攻坚的勇气是他们力量的源泉，这就是建筑人生的追求!<br /></font></p>
                        </blockquote></td>
                    </tr>
                </tbody>
            </table>
            </td>
        </tr>
    </tbody>
</table>]]>
</content>
</entry>

<entry>
<title>中国十大名茶</title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1563726.html"/>
<issued>2008-03-20T15-24-00 GMT+08:00</issued> 
<created>2008-03-20T15-24-00 GMT+08:00</created>
<modified>2008-08-22T09-12-33Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1563726</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>生活百科</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<table cellspacing="0" cellpadding="0" width="95%" align="center" border="0">
    <tbody>
        <tr>
            <td class="tit" align="center" height="50"><span class="STYLE16"><strong><font size="4">中国十大名茶</font></strong></span></td>
        </tr>
        <tr>
            <td class="tit" style="BORDER-BOTTOM: #666666 1px solid" align="center" height="30">发布时间：2007-12-8 阅读：<font color="#ff0000">28</font> 次 【字体：<a class="black" href="javascript:fontZoom(16)"><font face="Verdana" color="#000066">大</font></a> <a class="black" href="javascript:fontZoom(14)"><font face="Verdana" color="#000066">中</font></a> <a class="black" href="javascript:fontZoom(12)"><font face="Verdana" color="#000066">小</font></a>】</td>
        </tr>
        <tr>
            <td class="black" id="fontzoom"><br />1．西湖龙井 <br />　　是我国的第一名茶，产于浙江杭州西湖的狮峰、龙井、五云山、虎跑一带，历史上曾分为&ldquo;狮、龙、云、虎&rdquo;四个品类，其中多认为以产于狮峰的品质为最佳。龙井素有&ldquo;色绿、香郁、味醇&nbsp;、形美&rdquo;四绝著称于世。形光扁平直，色翠略黄似糙米色，滋味甘鲜醇和，香气幽雅清高，汤色碧绿黄莹；叶底细嫩成朵。&nbsp; <br /><br />2．洞庭碧螺春 <br />　　产于江苏吴县太湖之滨的洞庭山。碧螺春茶叶用春季从茶树采摘下的细嫩芽头炒制而成；高级的碧螺春，每公斤干茶需要茶芽13.6~15万个。外开形条索紧结，白毫显露，色泽银绿，翠碧诱人，卷曲成螺，故名&ldquo;碧螺春&rdquo;。汤色清澈明亮，浓郁甘醇，鲜爽生津，回味绵长；叶底嫩绿显翠。&nbsp; <br /><br />3．白毫银针 <br />　　素有茶中&ldquo;美女&rdquo;、&ldquo;茶王&rdquo;之美称，是一种白茶，产于福建东部的福鼎和北部的政和等地。&nbsp;白毫银针满坡白毫色白如银，细长如针，因而得名。冲泡时，&ldquo;满盏浮茶乳&rdquo;，银针挺立，上下交错，非常美观；汤色黄亮清澈，滋味清香甜爽。白茶味温性凉，为健胃提神，祛湿退热，常作为药用。&nbsp; <br /><br />4．君山银针&nbsp;&nbsp;&nbsp; <br /><br />&nbsp;&nbsp;&nbsp;&nbsp;产于岳阳洞庭湖的青螺岛，有&ldquo;洞庭帝子春长恨，二千年来草更长&rdquo;的描写。其冲泡后，三起三落，雀舌含珠，刀丛林立。很高的欣赏价值。&nbsp; <br /><br />5．&nbsp;黄山毛峰 <br />　　产于安徽黄山，主要分布在桃花峰的云谷寺、松谷庵、吊桥阉、慈光阁及半寺周围。这里山高林密，日照短，云雾多，自然条件十分优越，茶树得云雾之滋润，无寒暑之侵袭，蕴成良好的品质。黄山毛峰采制十分精细。制成的毛峰茶外形细扁微曲，状如雀舌，香如白兰，味醇回甘。&nbsp; <br /><br />6．&nbsp;武夷岩茶 <br />　　产于福建武夷山。武夷岩茶属半发酵茶，制作方法介于绿茶与红茶之间。其主要品种有&ldquo;大红袍&rdquo;、&ldquo;白鸡冠&rdquo;、&ldquo;水仙&rdquo;、&ldquo;乌龙&rdquo;、&ldquo;肉桂&rdquo;等。武夷岩茶品质独特，它未经窨花，茶汤却有浓郁的鲜花香，饮时甘馨可口，回味无穷。18世纪传入欧洲后，倍受当地群从的喜爱，曾有&ldquo;百病之药&rdquo;美誉。&nbsp; <br /><br />7．&nbsp;安溪铁观音 <br />　　产于福建安溪，铁观音的制作工艺十分复杂，制成的茶叶条索紧结，色泽乌润砂绿。好的铁观音，在制作过程中因咖啡碱随水分蒸发还会凝成一层白霜；冲泡后，有天然的兰花香，滋味纯浓。用小巧的工夫茶具品饮，先闻香，后尝味，顿觉满口生香，回味无穷。近年来，发现乌龙茶有健身美容的功效后，铁观音更风靡日本和东南亚。&nbsp; <br /><br />8．信阳毛尖&nbsp;&nbsp;&nbsp; <br /><br />&nbsp;&nbsp;&nbsp;&nbsp;产于河南信阳车云山、集云山、天云山、云雾山、震雷山、黑龙潭和白龙潭等群山峰顶上，以车云山天雾塔峰为最。人云：&ldquo;师河中心水，车云顶上茶。&rdquo;成品条索细圆紧直，色泽翠绿，白毫显露；汤色清绿明亮，香气鲜高，滋味鲜醇；叶底芽壮、嫩绿匀整。&nbsp; <br /><br />9．&nbsp;庐山云雾 <br />　　产于江西庐山。号称&ldquo;匡庐秀甲天下&rdquo;的庐山，北临长江，南傍鄱阳湖，气候温和，山水秀美十分适宜茶树生长。庐山云雾芽肥毫显，条索秀丽，香浓味甘，汤色清澈，是绿茶中的精品。&nbsp; <br /><br />10．六安瓜片 <br />　　产于皖西大别山茶区，其中以六安、金寨、霍山三县所产品最佳。六安瓜片每年春季采摘，成茶呈瓜子形，因而得名，色翠绿，香清高，味甘鲜，耐冲泡。此茶不仅可消暑解渴生津，而且还有极强的助消化作用和治病功效，明代闻龙在《茶笺》中称，六安茶入药最有功效，因而被视为珍品。&nbsp; <br /><br />　　在其它的&ldquo;中国十大名茶&rdquo;说法中，一般常见到产于安徽祁门县的&ldquo;祁红&rdquo;、产于云南的&ldquo;滇红&rdquo;&nbsp;湖北产&ldquo;恩施玉露&rdquo;产于云南西双版纳&ldquo;普洱茶&rdquo;&nbsp;等。</td>
        </tr>
        <tr align="right">
            <td>&nbsp;</td>
        </tr>
    </tbody>
</table>]]>
</content>
</entry>

<entry>
<title>茶也“醉”人吗？</title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1563721.html"/>
<issued>2008-03-20T15-22-55 GMT+08:00</issued> 
<created>2008-03-20T15-22-55 GMT+08:00</created>
<modified>2008-08-22T06-21-12Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1563721</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>生活百科</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<br />
<p>　　并非只有酒才能醉人，茶也能醉人。古人云，&ldquo;寒夜客来茶当酒。&rdquo;而&ldquo;茶醉&rdquo;比之&ldquo;酒醉&rdquo;，又别是一种境界。<br /><br />　　&ldquo;茶醉&rdquo;通常是因空腹饮茶、或是饮用了过浓、过多的茶所致。特征为面色苍白、欲吐、心悸、头晕、<a href="http://www.yok.com/go2.php?Key=失眠&amp;NO=8&amp;PID=9999_9999&amp;UN=100000007&amp;Times=7" target="_blank"><font color="#0000ff">失眠</font></a>、烦躁、乏力、腹痛红茶尤甚，以及短期厌食等。<br /><br />茶叶中含有多种生物碱，其中的主要成份是咖啡碱。它在茶叶中的含量约占２－５％，具有兴奋大脑神经中枢和促进心脏机能亢进的作用。如饮茶过浓、过多，就容易出现&ldquo;茶醉&rdquo;。<br /><br />　　&ldquo;茶醉&rdquo;除咖啡碱的作用外，还因为茶叶中含有大量茶多酚。它是一种多酚类物质，对蛋白质有凝固作用。因此，暴饮浓茶会妨碍胃液的正常分泌，影响食物的消化，于是就会出现醉茶现象。<br /><br />　　一旦发生&ldquo;茶醉&rdquo;，可以吃一、二颗糖果或是喝一些开水，这样，&ldquo;醉情&rdquo;能够得到一定的缓解。</p>]]>
</content>
</entry>

<entry>
<title>每杯茶冲泡几次</title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1563716.html"/>
<issued>2008-03-20T15-21-45 GMT+08:00</issued> 
<created>2008-03-20T15-21-45 GMT+08:00</created>
<modified>2008-08-22T09-12-33Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1563716</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>生活百科</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<table cellspacing="0" cellpadding="0" width="95%" align="center" border="0">
    <tbody>
        <tr>
            <td class="black" id="fontzoom">
            <p>　每杯茶的冲泡次数，由茶叶的种类和饮用方式而定。劣茶叶的耐泡程度，与茶叶的嫩度和加工后茶叶的完整性密切相关。加工越细碎的，越容易使茶汁冲泡出来；越粗老完整的茶叶，茶汁冲泡出来的速度越慢。<br /><br />　　饮用红碎茶，尤其是袋泡茶，一般只冲泡1次，不再泡第2次。因红碎茶粒度细，冲泡时茶汁易于浸出。一般的条形绿茶，如炒青眉茶、花茶、龙井、乌龙茶等，因茶汁浸吐较慢，可冲泡2一3次。这些茶叶，第1次冲泡浸出量占可溶物总量的55%左右，第2次冲泡浸出量占30%左右，第3次为10%左有，而第4次只有1%&mdash;&mdash;3%。从营养角度看，茶中的维生素C、氨基酸和多种无机物等，第l次冲泡就有80%被浸出，第2次冲泡有95%以上被溶出；从茶多酚、咖啡碱等药效成分溶出看，第1次冲泡浸出率最大，经3次冲泡后基本达到全量浸出。就茶汤的色香滋味而言，不少饮茶者有如下体：一泡茶香味鲜爽，二泡茶虽浓涩但不鲜，三泡已淡薄，四泡无滋味，五泡、六泡等于饮白开水。因此，无论从哪个角度看，每杯茶冲泡次数不宜太多。早上泡的一杯茶，反复冲泡，一直喝到晚上，那是不合适的。<br /><br />　　综上所述，一般红、绿、花茶，每杯茶冲泡次数，通常以3次为宜；乌龙茶，因冲泡时投茶量大，可冲泡3一5次；以红碎茶为原料的袋泡茶，茶汁易于浸出，通常适宜一次性冲泡</p>
            </td>
        </tr>
        <tr align="right">
            <td>&nbsp;</td>
        </tr>
    </tbody>
</table>]]>
</content>
</entry>

<entry>
<title>学会变通</title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1554201.html"/>
<issued>2008-03-18T20-10-42 GMT+08:00</issued> 
<created>2008-03-18T20-10-42 GMT+08:00</created>
<modified>2008-08-22T06-21-12Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1554201</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>优惠促销</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<div style="MARGIN-LEFT: 15px"><font style="FONT-SIZE: 10pt" color="#333333">爹对儿子说，我想给你找个媳妇。 <br />儿子说，可我愿意自己找！ <br />爹说，但这个女孩子是比尔盖茨的女儿！ <br />儿子说，要是这样，可以。 <br />然后他爹找到比尔盖茨，说，我给你女儿找了一个老公。 <br />比尔盖茨说，不行，我女儿还小！ <br />爹说，可是这个小伙子是世界银行的副总裁！ <br />比尔盖茨说，啊，这样，行！ <br />最后，爹找到了世界银行的总裁，说，我给你推荐一个副总裁！ <br />总裁说，可是我有太多副总裁了，多余了！ <br />爹说，可是这个小伙子是比尔盖茨的女婿！ <br />总裁说，这样呀，行！ <br />----生意就是这样做成的<br />看了这个故事，感悟很深，生活中的许多事，确实需要变通，往往看似牛马不相及的事情，往往转换个角度，就会柳暗花明又一村，生活是这样，工作同样也是！！</font></div>]]>
</content>
</entry>

<entry>
<title>如何管理应收帐款和催收货款</title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1321401.html"/>
<issued>2008-01-03T14-25-16 GMT+08:00</issued> 
<created>2008-01-03T14-25-16 GMT+08:00</created>
<modified>2008-08-22T06-21-13Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1321401</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>销售心得</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<div class="p_entry2" id="textboxContent">一、&nbsp;在销售合同中明确各项条款&nbsp;<br /><br />　　在与经销商签订销售合同时，要注意以下事项，以避免日后处理应收帐款时与经销商产生分歧而带来经营风险：&nbsp;<br />　　1、&nbsp;明确各项交易条件，如：价格、付款方式、付款日期、运输情况等；&nbsp;<br />　　2、&nbsp;明确双方的权利和违约责任；&nbsp;<br />　　3、&nbsp;确定合同期限，合同结束后视情况再行签订；&nbsp;<br />　　4、&nbsp;加盖经销商的合同专用章（避免个体行为的私章或签字）；&nbsp;<br /><br />　　二、&nbsp;定期的财务对帐&nbsp;<br /><br />　　财务要形成定期的对帐制度，每隔三个月或半年就必须同经销商核对一次帐目，以下几种情况容易造成单据、金额等方面的误差，厂家要尤为重视：&nbsp;<br />　　1、&nbsp;产品结构为多品种、多规格；&nbsp;<br />　　2、&nbsp;产品的回款期限不同，或因经营条件的不同而同种产品回款期限不同；&nbsp;<br />　　3、&nbsp;产品出现平调、退货、换货时；&nbsp;<br />　　4、&nbsp;经销商不能够按单对单（销售单据或发票）回款；&nbsp;<br />　　5、&nbsp;要主动拒绝用货款垫支其它款项（客户返利、破损产品货款、广告款、终端销售推广费用等）；&nbsp;<br />　　以上情况会给应收帐款的管理带来困难，因此要制订一套规范的、定期的对帐制度，避免双方财务上的差距像滚雪球一样越滚越大，而造成呆、死帐现象，同时对帐之后要形成具有法律效应的文书，而不是口头承诺。&nbsp;<br /><br />　　三、&nbsp;对产品铺货率的正确理解&nbsp;<br /><br />　　如果产品铺货率提高，会增加销售机会(提高了消费者的购买便利性)，但应收帐款和经营风险也同时增加；如果降低铺货率，经营风险虽然降低了，但达不到规模销售的目标。所以正确、合理的解决产品铺货率问题，对降低应收帐款，保证货款的安全性是有帮助的。因此我们建议在产品不同销售阶段、或根据产品不同的销售策略、或根据市场推广的强弱势而采取不同的产品铺货政策。&nbsp;<br /><br />　　四、&nbsp;减少赊销、代销运作方式&nbsp;<br /><br />　　销售人员为了迅速占领市场，或为了完成销售目标而采取赊销、代销的运作模式。这种销售模式是经销商拖欠应收货款的土壤，并极易造成呆、死帐的出现。我们要制订相应的销售奖励政策，鼓励经销商采取购销、现款现货等方式合作，尽量减少赊销、代销的方式。<br /><br />　　五、&nbsp;制定合理的激励政策&nbsp;<br /><br />　　我们在制定营销政策时，要将应收帐款的管理纳入对销售人员考核的项目之中，即个人利益不仅要和销售、回款业绩挂钩，也要和应收帐款的管理联系在一起，制订合理的应收帐款奖罚条例，使应收帐款处在合理、安全的范围之内。&nbsp;<br /><br />　　六、&nbsp;建立信用评定、审核制度&nbsp;<br /><br />　　在实际工作中，真正能够做到现款现货的经销商很少，我们要建立信用评定、审核制度，对不同的经销商给予不同的信用额度和期限（一般为半年）。对经销商的信用管理要采取动态的管理办法，即每半年根据前期合作情况，对经销商的信用情况重新评定。&nbsp;<br />经销商的监管<br /><br />　　一、&nbsp;建立完善的经销商开户制度&nbsp;<br /><br />　　当厂家开拓新的市场或对目标市场进行细分时，对经销商选择时进行充分、科学的评估是必要的，这不仅为将来的销售寻找一个合作伙伴，同时也降低了日益激烈的市场竞争所带来的经营风险。当我们面对着&ldquo;买方市场&rdquo;这个实际情况时，这是一个事半功倍的工作。&nbsp;<br />　　因此，合作前对经销商进行评估就显得尤为重要。评估的内容应包括：&nbsp;<br />　　1、&nbsp;经销商的资信状况；&nbsp;<br />　　包括：企业发展状况、在行业中的口碑、历史交易记录、在销售通路中上、下游的评价等。&nbsp;<br />　　2、&nbsp;经销商的财务状况；&nbsp;<br />　　包括：企业的性质、注册资金、资金来源、固定资产、流动资金、企业欠债情况、还债能力、经销商应收帐款等。&nbsp;<br />　　3、&nbsp;经销商的经营状况；&nbsp;<br />　　包括：公司发展方向、负责人经营理念、主营销售渠道、是否有本行业的经验、是否有经销竞争产品、是否有代理畅销产品、销售队伍、销售规模、仓储、物流配送系统等。&nbsp;<br />　　4、&nbsp;负责人的个人资料；&nbsp;<br />　　包括：社会地位、家庭背景、个人背景、家庭成员、婚姻状况、个人爱好、不良嗜好等。&nbsp;<br /><br />　　二、&nbsp;对已合作经销商的监管：&nbsp;<br /><br />　　1、&nbsp;强化经销商的回款意识；&nbsp;<br />　　经销商在处理应付帐款时，会根据以下的原则而选择先后支付顺序：&nbsp;<br />　　a、&nbsp;对经销商利润贡献的多少；&nbsp;<br />　　b、&nbsp;代理产品销售金额的多少&nbsp;<br />　　c、&nbsp;代理产品在经销商心目中的地位；&nbsp;<br />　　d、&nbsp;客情关系的维护程度；&nbsp;<br />　　e、&nbsp;厂家对货款管理的松、紧程度；&nbsp;<br />　　要经常性地强化经销商的回款意识，将本公司的付款顺序排列在前面，成为经销商的第一付款顺序是我们的目标和努力方向。&nbsp;<br />　　2、&nbsp;控制发货以减少应收帐款；&nbsp;<br />　　按照经销商实际的经营情况，采用&ldquo;多批少量&rdquo;的方法可以有效地控制应收帐款。根据个人以往经验，以每月发货1～2次为宜，即每次发货量为经销商15～30日的销售量。&nbsp;<br />　　3、&nbsp;适当的通路促销以减少应收帐款；&nbsp;<br />　　根据20／80原则，对于20％这部分重点客户的应收帐款的管理，是应收款管理的重中之重。实行通路促销政策，可以有效地降低厂家的应收帐款。但此种方式应谨慎使用，不宜过濒（一年一次为宜）。同时建议：在年中以通路促销为条件、在年末以年终返利为条件促使重点大客户降低应收帐款。&nbsp;<br />　　4、&nbsp;建立经销商的库存管理制度；&nbsp;<br />　　通过对经销商库存的动态管理（销售频率、销售数量、销售通路、覆盖区域等），及时了解经销商的经营状况，保证销售的正常运转，有效地控制应收帐款。&nbsp;<br /><br />　　三、&nbsp;经销商发生欠款的危险信号：<br />　　在日常经营、管理中，经销商出现的一些信息，对厂家货款的安全性是有警示作用的。如：&nbsp;<br />　　1.&nbsp;办公地点由高档向低档搬迁；&nbsp;<br />　　2.&nbsp;频繁转换管理层、业务人员，公司离职人员增加；&nbsp;<br />　　3.&nbsp;受到其他公司的法律诉讼；&nbsp;<br />　　4.&nbsp;公司财务人员经常性的回避；&nbsp;<br />　　5.&nbsp;付款比过去延迟；经常超出最后期限；&nbsp;<br />　　6.&nbsp;多次破坏付款承诺；&nbsp;<br />　　7.&nbsp;经常找不到公司负责人；&nbsp;<br />　　8.&nbsp;公司负责人发生意外；&nbsp;<br />　　9.&nbsp;公司决策层存在较严重的内部矛盾，未来发展方向不明确。&nbsp;<br />　　10.&nbsp;公司有其他的不明确赢利的投资（投机）如：股票、期货等；&nbsp;<br />　　11.&nbsp;不正常的不回复电话；&nbsp;<br />　　12.&nbsp;开出大量的期票；&nbsp;<br />　　13.&nbsp;银行退票（理由：余款不足）；&nbsp;<br />　　14.&nbsp;应收帐款过多，资金回笼困难；&nbsp;<br />　　15.&nbsp;转换银行过于频繁；&nbsp;<br />　　16.&nbsp;以低价抛售商品（低于供货商底价）&nbsp;<br />　　17.&nbsp;突然下过大的定单（远远超出所在区域的销售能力）；&nbsp;<br />　　18.&nbsp;发展过快（管理、经营不能同步发展）；&nbsp;<br />　　当经销商出现以上危险信息时，厂家采取果断、迅速的应变措施，可以降低应收帐款的回收风险。&nbsp;<br />&nbsp;&nbsp;销售人员的监管<br />&nbsp;&nbsp;&nbsp;&nbsp;拖欠时间（月）&nbsp;1&nbsp;2&nbsp;3&nbsp;6&nbsp;9&nbsp;12&nbsp;24<br />&nbsp;&nbsp;&nbsp;&nbsp;成功率&nbsp;93％&nbsp;85％&nbsp;73％&nbsp;57％&nbsp;42％&nbsp;25％&nbsp;13％<br /><br />　　一、&nbsp;加强销售人员的原则性：&nbsp;<br />　　在实际的销售管理过程中，我们会感觉到销售人员总是帮助经销商向厂家索要更多的利益。销售人员如何处理厂家与经销商的关系是一个重要的课题。我们经常听到：&ldquo;厂家和经销商要达到共赢&rdquo;，可是要真正做到这一点谈何容易。所以销售人员在同经销商维持良好的客情关系的同时，一定要加强他们的原则性，也就是销售人员的同情心和职业道德之间的关系，不折不扣的执行公司制定的销售政策（应收帐款管理）。&nbsp;<br /><br /><br />　　二、&nbsp;加强销售人员的回款意识：&nbsp;<br />　　我们应该销售人员培养成良好的习惯：货款回收期限前一周，电话通知或拜访负责人，预知其结款日期；期限前三天确定结款日期，如自己不能如约应通知对方自己的某一位同事会前往处理，如对方不能如约应建议对方授权其他人跟进此款；在结款日一定按时前往拜访。&nbsp;<br />　　1、&nbsp;因为时间是欠款者的保护伞，时间越长，追收成功率越低：&nbsp;<br />　　2、&nbsp;最后收款期限&nbsp;<br />　　a、&nbsp;客户拖欠之日数，不应超过回款期限的1/3；如超过，应马上采取行动追讨；&nbsp;<br />　　b、&nbsp;如期限是30天，最后收款期限不能超过40天；&nbsp;<br />　　c、&nbsp;如期限是60天，最后收款期限不能超过80天；&nbsp;<br />　　d、&nbsp;如果不马上追讨，相当于将回款的机会让给别的公司，同时本公司的经营风险就相应的提高。&nbsp;<br /><br />　　三、&nbsp;加强销售人员终端管理、维护能力：&nbsp;<br />　　建立一套行之有效的终端维护的管理办法，不仅可以降低经销商的经营风险，确保厂家货款的安全；同时也可以提升销售业绩，提高公司形象、产品形象在经销商中的地位，这对及时清欠应收帐款都是有益的。&nbsp;<br />　　我们要记住：&nbsp;<br />　　要确保厂方的销售回款，就要确保经销商的销售回款。&nbsp;<br />　　要厂家的生意提高，就要确保经销商的生意。&nbsp;<br /><br />　　四、&nbsp;提高销售人员追款技巧：<br />　　销售人员在成功追收帐款中扮演着很重要的角色，在日常工作中要加强销售人员在这方面的培训：&nbsp;<br />　　1.&nbsp;运用常识；&nbsp;<br />　　2.&nbsp;追讨函件；&nbsp;<br />　　3.&nbsp;丰富、完善的客户资料档案；&nbsp;<br />　　4.&nbsp;让对方写下支付欠款的承诺函件，并加盖公章；&nbsp;<br />　　5.&nbsp;与负责人直接接触；&nbsp;<br />　　6.&nbsp;录音；&nbsp;<br />　　7.&nbsp;向警方求助；&nbsp;<br />　　8.&nbsp;谨慎从事；&nbsp;<br />　　9.&nbsp;丰富自己财务、银行等方面的知识。如：支票、电汇、汇票、承兑汇票、退票等。&nbsp;<br /><br />　　五、&nbsp;零售终端经营不善的危险信号：&nbsp;<br />　　在日常拜访中，检查零售终端的经营状况是终端代表重要工作之一，当终端出现下列状况时，我们就要特别的谨慎，应及时将此信息通报给经销商，避免经销商的经营损失：&nbsp;<br />　　1.&nbsp;正常的营运费用无法支付（如：房租、水电、工资）；&nbsp;<br />　　2.&nbsp;商场负责人无正当理由的突然失踪；&nbsp;<br />　　3.&nbsp;商场业务人员的频繁更换；&nbsp;<br />　　4.&nbsp;商品大打折扣（低于供应商的底价）；&nbsp;<br />　　5.&nbsp;频繁的有商家退出经营；&nbsp;<br />　　6.&nbsp;货架出现大量的空位；&nbsp;<br />　　7.&nbsp;大量使用礼品劵，抵供应商的货款；&nbsp;<br />　　8.&nbsp;大量的无法兑付的空头支票；&nbsp;<br />　　9.&nbsp;不正常的盘点；&nbsp;<br />　　10.&nbsp;商场没有人气；<br /><br />&nbsp;&nbsp;&nbsp;&nbsp;成功追收应付帐款<br />　　一、&nbsp;应收帐款的处理方法&nbsp;<br />　　1.&nbsp;销售资料（收货单据、发票等）是否齐备？内容是否准确无误？&nbsp;<br />　　2.&nbsp;准时给予文件；其实越早给经销商发票，货款回收可能越早，同时要确认经销商收到发票；&nbsp;<br />　　3.&nbsp;完善客户跟进制度：客户接触率与成功回收率是成正比的，越早与客户接触，与客户开诚布公的沟通，被拖欠的机会越低；&nbsp;<br />　　4.&nbsp;定期探访：如客户到期付款，应按时上门收款，或电话催收；即使是过期一天，也应马上追收，不&nbsp;应有等待的心理；&nbsp;<br />　　5.&nbsp;建立形象：客户是需要教育的，一定要给予客户一个正确的观念：我们对所有欠款都是非常严肃的，是不能够容忍被拖欠的；&nbsp;<br />　　6.&nbsp;服务精神：认同及理解客户的困难和投诉，同时可以利用自身的优势帮助客户解决困难；&nbsp;<br />　　7.&nbsp;技巧训练：追收欠款是需要技巧的，如：电话技巧、上门拜访技巧；同时应了解客户的经营状况、财务状况、个人背景等资料；&nbsp;<br /><br />　　二、&nbsp;已被拖欠款项的处理方法&nbsp;<br />　　1.&nbsp;文件：检查被拖欠款项的销售文件是否齐备&nbsp;<br />　　2.&nbsp;收集资料：要求客户提供拖欠款项的原因，并收集资料以证明其正确性；&nbsp;<br />　　3.&nbsp;追讨文件：建立帐款催收制度。根据情况发展的不同，建立三种不同程度的追讨文件――预告、警告、律师信，按情况及时发出；&nbsp;<br />　　4.&nbsp;最后期限：要求客户了解最后的期限以及其后果，让客户了解最后期限的含义；&nbsp;<br />　　5.&nbsp;行动升级：将欠款交予较高级的管理人员处理，将压力提升；&nbsp;<br />　　6.&nbsp;假起诉：成立公司内部的法律部，以法律部的名义发出追讨函件，警告容忍已经到最后期限；&nbsp;<br />　　7.&nbsp;调节：使用分期付款、罚息、停止数期等手段分期收回欠款；<br />　　8.&nbsp;要求协助：使用法律维护自己的利益。&nbsp;<br /><br />　　三、&nbsp;对于呆/死帐的处理方法：&nbsp;<br />　　1.&nbsp;折让&nbsp;<br />　　2.&nbsp;收回货物&nbsp;<br />　　3.&nbsp;处理抵押品&nbsp;<br />　　4.&nbsp;寻求法律协助&nbsp;<br />　　5.&nbsp;诉讼保全<br /></div>]]>
</content>
</entry>

<entry>
<title>《能源法》向公众征集意见 蕴育新机</title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1240518.html"/>
<issued>2007-12-06T20-45-11 GMT+08:00</issued> 
<created>2007-12-06T20-45-11 GMT+08:00</created>
<modified>2008-08-22T09-12-33Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1240518</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>Default Cloumn</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<p><span class="style2">国家能源办在其网站（<a href="http://www.chinaenergy.gov.cn/">www.chinaenergy.gov.cn</a>）公布了《能源法》（征求意见稿），并表示，为进一步提高立法工作的<nobr oncontextmenu="return false;" onmousemove="kwM(0);" id="key0" onmouseover="kwE(event,0, this);" onclick="return kwC();" onmouseout="kwL(event, this);" target="_blank">科学</nobr>性、民主性和透明度，《能源法》起草组决定从2007年12月1日开始，通过新闻媒体和互联网等渠道向社会各界广泛征集修改、完善的意见和建议。此次征求意见活动计划至2008年2月1日结束。<br /><clk></clk>《能源法》是我国能源领域的基础性法律，目前公布的《能源法》（征求意见稿）共分为十五章，囊括了能源综合管理、战略与规划、<nobr oncontextmenu="return false;" onmousemove="kwM(1);" id="key1" onmouseover="kwE(event,1, this);" onclick="return kwC();" onmouseout="kwL(event, this);" target="_blank">开发</nobr>与加工转换、供应与服务、能源节约、能源储备、能源应急、农村能源、能源价格与财税、能源科技以及能源国际合作等诸多内容。对于社会各界比较关注的能源管理部门的设置，&ldquo;征求意见稿&rdquo;中并未提到具体名称，但规定&ldquo;国务院能源主管部门统一管理全国能源工作，国务院其他有关部门在各自职责范围内负责相关能源管<nobr oncontextmenu="return false;" onmousemove="kwM(2);" id="key2" onmouseover="kwE(event,2, this);" onclick="return kwC();" onmouseout="kwL(event, this);" target="_blank">理工</nobr>作&rdquo;。<br /><clk></clk>为了鼓励节约能源，&ldquo;征求意见稿&rdquo;在能源价格和税收政策上做了详细规定。<br />关于能源价格形成机制，&ldquo;征求意见稿&rdquo;提出，国家建立市场调节与政府调控相结合、以市场调节为主导的能源价格形成机制。其中，对于&ldquo;具备市场竞争条件的能源产品和服务价格，实行市场调节价&rdquo;；对于自然垄断经营的能源输送管网的输送价格及关系公共利益的重要能源产品和服务价格，实行<nobr oncontextmenu="return false;" onmousemove="kwM(10);" id="key4" onmouseover="kwE(event,10, this);" onclick="return kwC();" onmouseout="kwL(event, this);" target="_blank">政府</nobr>定价或者政府指导价，并逐步推行有利于降低成本、提高效率、节约资源和减少环境损害的价格管制制度。在价格激励与约束政策方面，&ldquo;国家鼓励发展的风能、太阳能、生物质能等可再生能源和新能源，依法实行激励型的价格政策。对国家限制发展的高耗能、高污染的企业、产品和服务，依法实行约束型的能源价格政策。<br />在能源税收激励政策方面，&ldquo;征求意见稿&rdquo;提出，&ldquo;国家运用税收政策鼓励新能源和可再生能源的开发利用，支持能源清洁利用和发展替代能源，支持节能产品和节能设备的生产应用和技术推广，鼓励进口<nobr oncontextmenu="return false;" onmousemove="kwM(3);" id="key3" onmouseover="kwE(event,3, this);" onclick="return kwC();" onmouseout="kwL(event, this);" target="_blank">优质</nobr>能源产品和能源开发利用必需的先进设备和技术。&rdquo;<br />期待明年2月份新《能源法》，期待《能源法》蕴育成熟，希望能够给能源相关行业带来更大的商机。<br /></span></p>
<div><img style="WIDTH: 1px; HEIGHT: 15px" alt="" src="http://www.topenergy.org/data/skins/chinese/images/blank.gif" border="0" /></div>]]>
</content>
</entry>

<entry>
<title>外墙外保温无秩序发展 是节能还是浪费<转></title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1219845.html"/>
<issued>2007-11-29T21-20-16 GMT+08:00</issued> 
<created>2007-11-29T21-20-16 GMT+08:00</created>
<modified>2008-08-22T06-21-13Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1219845</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>Default Cloumn</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<p><font face="Courier">今年全国范围开始的外墙外保温建设热更像一场无组织的运动，没有统一的实施方案，没有统一的执行标准，各地方、各企业各自为政&hellip;&hellip;这场以节能为目的的运动，正在成为浪费大战，浪费资金，浪费资源，污染环境&hellip;&hellip;&rdquo;江苏某总裁痛心地说。</font></p>
<p><font face="Courier">　　2007年可以说是外墙外保温年，在政府关于建设节约型社会的倡导下，在2006年国务院下发节能减排综合性工作方案的通知后，建筑节能逐渐在全国范围内普及，并不断推向高潮，全国各地建设厅和建委纷纷出台政策规定新建建筑必须进行墙体保温，某些省份甚至规定房地产项目达到保温规定方可进行竣工验收。节能建筑似乎离我们越来越近。</font></p>
<p><font face="Courier">　　然而，事实并非如此。今年开始的全国墙体保温热已演变成了一场运动，或者说是一场淘金游戏。背后的隐忧不能不让人担心。</font></p>
<p><font face="Courier">　　隐忧一：一场没有游戏规则的游戏目前，国家没有墙体保温的法规，没有统一的实施和验收标准，各地方各自为政。百代新材的沈阳介绍说：&ldquo;目前市场主要以外墙外保温技术为主，内墙保温由于占用建筑面积大和效果差基本被淘汰，而外墙外保温技术又有EPS板薄抹灰系统、胶粉聚苯颗粒保温浆料系统、EPS板现浇系统、EPS钢丝网架板现浇混凝土系统、保温板与装饰一体化成型安装系统、聚氨脂现场喷涂复合聚苯乙烯颗粒找平系统、砌体结构夹芯保温墙体系统等多种技术体系。这些体系各有优缺点，无论是专家还是各级政府主管部门，均难以达成一致的意见，也不能形成统一的标准。因此有些企业实施起来难免不混水摸鱼，只考虑自己的利益而不考虑节能效果。实际上这种状况也不利于整个市场的健康发展。目前，市场上大约有大大小小的外墙外保温生产厂家3000多家，竞争激烈，市场极不规范。就保温砂浆而言，有8000多元一吨的，也有500元一吨的，500元一吨的恐怕全是沙子了，能不能达到保温效果只有天知道！&rdquo;由此可见，国家出台外墙外保温体系的规范法规已迫在眉睫。</font></p>
<p><font face="Courier">　　隐忧二：一场淘金者的游戏尽管没有统一的法规，但对于各种外墙外保温体系，各地政府均有自己的检测标准，并把它作为创收来源，山东某墙体保温材料厂的刘总对此有一肚子苦水：从去年开始投资外墙外保温系统，目前已进入14个城市，但光进入这14个城市的检测办证费用就花了100万元，一个系统，每进入一个市场，需要的检测准入费用从2万元到8万元不等。</font></p>
<p><font face="Courier">　　而各生产外墙外保温材料的厂家，更是鱼龙混杂，甚至有不少家庭作坊式的企业加入其中，市场才刚刚预热，就陷入天昏地暗的价格战之中，大企业无法生存，小企业却能淘金，留下的是很多建筑隐患。比如保温板与装饰一体化成型安装系统，要达到好的装饰和保温效果，每平方米的造价应该在300元左右，但同一项目招标中，有的企业却报出150元的价格，使业主无从选择。目前，恶劣的生存环境使外墙外保温行业还没有出现一个知名品牌。</font></p>
<p><font face="Courier">　　隐忧三：节能还是浪费目前的外墙外保温乱象，其明显的危害是达不到保温效果，不利于行业的发展，浪费了资金和资源。但最大的危害还是它的隐性危害，即环保隐患。就目前的外墙外保温市场而言，其中有一半以上将达不到保温效果，甚至在3~5年时间内会出现开裂、脱落等现象，更不要说能达到25年的寿命。可以断言，其中50%以上连10年的寿命都达不到。可怕的是，10年内产生的建筑垃圾将以数百亿吨计，其中有多少是污染环境的聚苯材料？将来我们又如何处理这些建筑垃圾？</font></p>
<p><font face="Courier">　　涂料行业热衷于搞保温装饰一体化的企业近年来有不断增加的趋势，面对这些隐忧，你们该如何办？</font></p>]]>
</content>
</entry>

<entry>
<title>EPS外保温用的胶粘剂和抹面胶浆</title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1219806.html"/>
<issued>2007-11-29T20-58-32 GMT+08:00</issued> 
<created>2007-11-29T20-58-32 GMT+08:00</created>
<modified>2008-08-22T06-21-14Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1219806</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>Default Cloumn</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[<p><strong><font face="Courier">EPS外保温用的胶粘剂和抹面胶浆</font></strong></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 近些年来，节能建筑外墙采用EPS外保温的工程越来越多，约占节能建筑的70%。这种保温除了要用18㎏/㎡的阻燃型聚苯乙烯发泡板、160ｇ/㎡的涂塑耐碱玻璃纤维网格布外，还要使用性能优良的胶粘剂和抹面胶浆。胶粘剂和抹面胶浆有胶液（双组份）型和干粉（单组份）型。干粉胶粘剂和抹面胶浆的参考配方如下：<br /></font></p>
<p>
<table cellspacing="0" cellpadding="0" border="1">
    <tbody>
        <tr>
            <td valign="top" width="175" rowspan="2">
            <div>&nbsp;&nbsp;&nbsp;&nbsp; &nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;&nbsp;项目</div>
            <div>材料</div>
            </td>
            <td valign="top" width="192">
            <div align="center">粘结胶粘剂</div>
            </td>
            <td valign="top" width="201">
            <div align="center">抹面胶浆</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="192">
            <div align="center">公斤</div>
            </td>
            <td valign="top" width="201">
            <div align="center">公斤</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>42.5级普通硅酸盐水泥</div>
            </td>
            <td valign="top" width="192">
            <div align="left">30</div>
            </td>
            <td valign="top" width="201">
            <div>28.5</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>石英砂</div>
            </td>
            <td valign="top" width="192">
            <div align="left">62.5(40～70目)</div>
            </td>
            <td valign="top" width="201">
            <div>56 (70～140目)</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>粉煤灰</div>
            </td>
            <td valign="top" width="192">
            <div align="left">4.5</div>
            </td>
            <td valign="top" width="201">
            <div>4.2</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>胶粉LDM1646P或GS2600</div>
            </td>
            <td valign="top" width="192">
            <div align="left">2.2</div>
            </td>
            <td valign="top" width="201">
            <div>1.7</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>胶粉DM200</div>
            </td>
            <td valign="top" width="192">
            <div align="left">0.5</div>
            </td>
            <td valign="top" width="201">
            <div>1.5</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>HPMC纤维素MH80000S</div>
            </td>
            <td valign="top" width="192">
            <div align="left">0.2</div>
            </td>
            <td valign="top" width="201">
            <div>0.3</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>甲酸钙（建筑用）</div>
            </td>
            <td valign="top" width="192">
            <div align="left">0.2</div>
            </td>
            <td valign="top" width="201">
            <div>0.2</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>矿物纤维</div>
            </td>
            <td valign="top" width="192">
            <div align="left">---</div>
            </td>
            <td valign="top" width="201">
            <div>3.5</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>易分散耐拉纤维（3-5mm）</div>
            </td>
            <td valign="top" width="192">
            <div align="left">---</div>
            </td>
            <td valign="top" width="201">
            <div>0.1</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>300-400目重钙粉</div>
            </td>
            <td valign="top" width="192">
            <div align="left">---</div>
            </td>
            <td valign="top" width="201">
            <div>2.5</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>轻钙粉</div>
            </td>
            <td valign="top" width="192">
            <div align="left">---</div>
            </td>
            <td valign="top" width="201">
            <div>1.5</div>
            </td>
        </tr>
        <tr>
            <td valign="top" width="175">
            <div>合计</div>
            </td>
            <td valign="top" width="192">
            <div align="left">100.1</div>
            </td>
            <td valign="top" width="201">
            <div>100</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; <strong>干粉胶粘剂和抹面胶浆的生产工艺和设备</strong></font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 2.0吨的干粉搅拌机一台(7.5KW电机),200㎏量程的台称一台,厂房200㎡(净高3.5ｍ以上),原料及成品库房200㎡。厂房和库房要防风、防雨。</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 生产时，按原材料品种、规格采购，严格按配方比计量，先开启搅拌机使其正常运转，分批循环投料，加完物料后，搅拌（20分钟左右）均匀，就可放料（出料的第一袋要投入加料口再搅拌），包装，最后停机。在干燥条件下的存放期为6个月。</font></p>
<p><font face="Courier">&nbsp;&nbsp; <strong>使用干粉胶粘剂和抹面胶浆</strong></font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 现场加水（先加适量水，再加干胶粉，总的水料比为0.20～0.25），用机械搅拌使之均匀,静置3～5分钟,再稍加搅拌就可使用；被保温的墙面要清理干净、平整。粘结保温板用胶粘剂，胶粘剂与基层的粘结面积应大于保温板面积的30%；抹面用抹面胶粉拌制的胶浆，先在已粘贴、锚固、平整的保温板上满抹抹面胶浆，再铺涂塑耐碱玻璃纤维网格布（搭接长度为5-10㎜），并把网格布压入胶浆中，干燥后再抹表面胶浆，面层胶浆的总厚度&le;5㎜。</font></p>]]>
</content>
</entry>

<entry>
<title>胶粉聚苯颗粒外墙外保温系统JG158—2004</title>
<link rel="alternate" type="text/html" href="http://www.bokee.net/blogmodule/weblogcomment_viewEntry/1219690.html"/>
<issued>2007-11-29T20-07-28 GMT+08:00</issued> 
<created>2007-11-29T20-07-28 GMT+08:00</created>
<modified>2008-08-22T06-21-14Z</modified>
<id>tag:cybx1118.blogchina.com,2005://1219690</id>
<author>
<name>cybx1118</name>
<url>http://www.bokee.net/blogmodule/weblogcomment_index/cybx1118.html</url>
</author>
<dc:subject>Default Cloumn</dc:subject>
<content type="text/html" mode="escaped" xml:lang="zh_CN" xml:base="http://www.bokee.net"> 
<![CDATA[前言<br /><br />　　本标准按照GB/T 1.1&mdash;2000《标准化工作导则 第1部分：标准的结构和编写规则》和GB/T 1.2&mdash;2002《标准化工作导则 第2部分：标准中规范性技术要素内容的确定方法》的规定编写。本标准非等效采用DIN 18550 第三部分《灰浆&mdash;&mdash;由矿物胶凝剂和聚苯乙烯泡沫塑料（EPS）作骨料制成的绝热灰泥》。根据我国国情，调整和增加了组成材料的部分技术性能指标。
<div align="left"><br />&nbsp;&nbsp;&nbsp; 在试验方法上，本标准非等效采用EIMA 101.86《外保温与装饰系统抗快速变形冲击标准试验方法》、EIMA 105.01《耐碱玻璃纤维增强网 外保温与装饰系统类》、ASTM D 968&mdash;1993《系统涂层下落法磨损测试耐磨性的标准试验方法》。</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;本标准5.1中&ldquo;面砖饰面外保温系统抗震性能应满足要求&rdquo;为强制性条款。<br />&nbsp;&nbsp;&nbsp;&nbsp;本标准的附录A、附录B、附录C、附录D、附录E、附录F、附录G、附录H为规范性附录。<br />&nbsp;&nbsp;&nbsp;&nbsp;本标准由建设部标准定额研究所提出。<br />&nbsp;&nbsp;&nbsp;&nbsp;本标准由建设部建筑制品与构配件产品标准化技术委员会归口。<br />&nbsp;&nbsp;&nbsp;&nbsp;本标准主要负责起草单位：北京振利高新技术公司、中国建筑标准设计研究所。</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;本标准参加起草单位：建设部科技发展促进中心、北京市恒岳新技术发展中心、中国建筑科学研究院物理所、中国建筑科学研究院工程抗震研究所、国家发展和改革委员会国家投资项目评审中心、北京建工集团有限责任公司、新疆建筑标准设计办公室、天津市建筑标准设计办公室、济南市墙体改革办公室、北京市昌平区建委、北京市第五建筑工程公司、北京市第六建筑工程公司、北京住总集团住一分部。</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;本标准主要起草人：黄振利、李晓明、杨西伟、方展和、冯金秋、程绍革、李东杰、王庆生、朱青、刘钢、陈平、王建康、李东毅、康伟、杜洪涛、陈丹林、朱晓伟、钱艳荣、陈全良、林燕成、何晓燕。</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;本标准为首次发布，自2003年 月 日起实施。<br /><br /><a name="2"></a><br />引 言<br /><br />　　本标准的发布机构提请注意如下事实，声明符合本标准时，可以使用涉及3.1条中有关&ldquo;胶粉聚苯颗粒外保温系统基本构造&rdquo;、5.7条及3.6条中有关&ldquo;耐碱网格布的孔径、表面涂覆抗碱保护膜及使用方法&rdquo;、3.4条中有关&ldquo;胶粉料与聚苯颗粒混凝成型构成保温层&rdquo;的相关专利。<br />已经识别出的专利：</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;发明专利&ldquo;抗裂保温墙体及施工工艺（专利号：ZL 98 1 03325.3 国际专利主分类号：E04C 2/284）&rdquo;</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;涉及胶粉聚苯颗粒外保温系统基本构造、材料配比包装及施工工艺；</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;实用新型专利：&ldquo;胶粉聚苯颗粒外保温粘贴面砖墙体（专利号：ZL02288982.5）&rdquo;涉及胶粉聚苯颗粒外保温粘贴面砖墙体的基本构造及锚固件在墙面上的分布固定方式等。</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;实用新型专利：&ldquo;塑料复合玻纤网格布（专利号：ZL98 207104.3）&rdquo;涉及耐碱玻纤网格布的表面保护膜涂覆技术及网格布孔径。</div>
<div align="left">&nbsp;本标准的发布机构对于专利的范围、有效性和验证资料不提出任何看法。<br />专利持有人已向本标准的发布机构保证，他愿意同任何申请人在合理和非歧视的条款和条件下，就使用授权许可证进行谈判。在这方面，该专利持有人的声明已在本标准的发布机构备案。有关资料可从以下地址获得：
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;上述专利的专利持有人：黄振利 北京振利高新技术公司 地址：北京丰台西局西街乙88号<br />电话：（010）63826971 E-mail:huangzhenli@yeah.net http://www.zhenli.com.cn<br />请注意除上述已经识别出的专利外，本标准的某些内容有可能涉及专利。本标准的发布机构不应承担识别这些专利的责任。<br /><br /><a name="3"></a>1.范围 </div>
<div align="left">&nbsp;</div>
<div align="left">&nbsp;&nbsp;&nbsp;&nbsp;本标准规定了胶粉聚苯颗粒外墙外保温系统的适用范围、术语和定义、分类和标记、技术要求、试验方法、检验规则、标志和标签以及产品的包装、运输和贮存。</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;本标准适用于以胶粉聚苯颗粒保温浆料为保温层、抗裂砂浆复合耐碱玻璃纤维网格布或热镀锌电焊网为防护层、涂料或面砖为饰面层的建筑物外墙外保温系统。<br /><br /><a name="4"></a>2.规范性引用文件 </div>
<div align="left">&nbsp;</div>
<div align="left">下列文件中的条款通过本标准的引用而成为本标准的条款。凡是注日期的引用文件，其随后所有的修改单(不包括勘误的内容)或修订版均不适用于本标准，然而，鼓励根据本标准达成协议的各方研究是否可使用这些文件的最新版本。凡是不注日期的引用文件，其最新版本适用于本标准。<br />GBJ 82&mdash;1985 普通混凝土长期性能和耐久性能试验方法<br />GB 175&mdash;1999 硅酸盐水泥、普通硅酸盐水泥<br />GB/T 1346&mdash;2001 水泥标准稠度用水量、凝结时间、安定性检验方法<br />GB/T 1728&mdash;1979 漆膜、腻子膜干燥时间测定法<br />GB 1748&mdash;1979 腻子膜柔韧性测定法<br />GB/T 2793－1995 胶粘剂不挥发物含量的测定<br />GB 3186 涂料产品的取样<br />GB/T 3810.1&mdash;1999 陶瓷砖试验方法 第1部分：抽样和接收条件（idt ISO 10545-1:1995）<br />GB/T 3810.2&mdash;1999 陶瓷砖试验方法 第2部分：尺寸和表面质量的检验（idt ISO 10545-2:1995）<br />GB/T 3810.3&mdash;1999 陶瓷砖试验方法 第3部分：吸水率、显气孔率、表观相对密度和容重的测定<br />（idt ISO 10545-3:1995）<br />GB/T 3810.12&mdash;1999 陶瓷砖试验方法 第12部分：抗冻性的测定（idt ISO 10545-12:1995）<br />GB/T 4100.1、GB/T 4100.2、 GB/T 4100.3、 GB/T 4100.4 干压陶瓷砖<br />GB/T 7689.3&mdash;2001 增强材料 机织物试验方法 第1部分宽度和长度的测定<br />GB/T 7689.5&mdash;2001 增强材料 机织物试验方法 第5部分玻璃纤维拉伸断裂强力和断裂伸长的测定<br />GB/T 7697 玻璃马赛克<br />GB/T 8625－1988 建筑材料难燃性试验方法<br />GB/T 9195 陶瓷砖和卫生陶瓷分类及术语<br />GB 9779&mdash;1988 复层建筑涂料<br />GB/T 9914.2&mdash;2001 增强制品试验方法 第2部分：玻璃纤维可燃物含量的测定<br />GB/T 9914.3&mdash;2001 增强制品试验方法 第3部分：单位面积质量的测定<br />GB/T 10294－1988 绝热材料稳态热阻及有关特性的测定 防护热板法<br />GB/T 16777&mdash;1997 建筑防水涂料试验方法<br />GB/T 17146&mdash;1997 建筑材料水蒸气透过性能试验方法<br />GB/T 17671&mdash;1999 水泥胶砂强度检验方法（ISO法）<br />GB 50011&mdash;2001 建筑抗震设计规范<br />GB 50178&mdash;1993 建筑气候区划标准<br />JC 209－1992 膨胀珍珠岩<br />JC 719 耐碱玻璃球<br />JC/T 457 陶瓷劈离砖<br />JC/T 547&mdash;1994 陶瓷墙地砖胶粘剂<br />JC/T 841&mdash;1999 耐碱玻璃纤维网格布<br />JGJ 51&mdash;2002 轻集料混凝土技术规程<br />JGJ 52&mdash;1992 普通混凝土用砂质量标准及检验方法<br />JGJ 70－1990 建筑砂浆基本性能试验方法<br />JGJ 101&mdash;1996 建筑抗震试验方法规程<br />JGJ 110&mdash;1997 建筑工程饰面砖粘结强度检验标准<br />JG/T 24&mdash;2000 合成树脂乳液砂壁状建筑涂料<br />JG 149&mdash;2003 膨胀聚苯板薄抹灰外墙外保温系统<br />JG/T 3049&mdash;1998 建筑室内用腻子<br />QB/T 3897&mdash;1999 镀锌电焊网<span class="px14"><font id="FontSizeSettings5">
<div></div>
<div align="left"><a name="5"></a>3.术语和定义 </div>
<div align="left">&nbsp;</div>
<div align="left">&nbsp;&nbsp;&nbsp; 下列术语和定义适用于本标准</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;3.1 胶粉聚苯颗粒外墙外保温系统(简称胶粉聚苯颗粒外保温系统) external thermal insulating rendering systems made of mortar with bonding powder and using expanded polystyrene granule as aggregate(英文缩写为ETIRS)<br />设置在外墙外侧，由界面层、胶粉聚苯颗粒保温层、抗裂防护层和饰面层构成，起保温隔热、防护和装饰作用的构造系统。<br />注：涂料饰面胶粉聚苯颗粒外保温系统基本构造见表1。面砖饰面胶粉聚苯颗粒外保温系统基本构造见表2。</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp;&nbsp;3.2 基层墙体 substrate<br />建筑物中起承重或围护作用的外墙体。 </div>
<div align="left">&nbsp;</div>
<p align="center"><img style="BORDER-RIGHT: #000000 1px solid; BORDER-TOP: #000000 1px solid; BORDER-LEFT: #000000 1px solid; BORDER-BOTTOM: #000000 1px solid" alt="胶粉聚苯颗粒外墙外保温系统" src="http://img.hc360.com/coatings/info/images/200706/p2061108.gif" border="0" /></p>
<p align="center"><img style="BORDER-RIGHT: #000000 1px solid; BORDER-TOP: #000000 1px solid; BORDER-LEFT: #000000 1px solid; BORDER-BOTTOM: #000000 1px solid" alt="胶粉聚苯颗粒外墙外保温系统" src="http://img.hc360.com/coatings/info/images/200706/p2061109.gif" border="0" /></p>
<p style="FONT-SIZE: 12px" align="left"><a href="http://info.coatings.hc360.com/PicnewsList/" target="_blank"><font style="FONT-SIZE: 12px"></font></a></p>
<p><font style="FONT-SIZE: 14px"></font><font face="Courier">&nbsp;3.3 界面砂浆 interface treating agent<br />由高分子聚合物乳液与助剂配制成的界面剂与水泥和中砂按一定比例拌合均匀制成的砂浆。 </font></p>
<p>&nbsp;</p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.4 胶粉聚苯颗粒保温浆料 bonding powder expanded polystyrene granule insulating material由胶粉料和聚苯颗粒组成并且聚苯颗粒体积比不小于80%的保温灰浆。</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.5 胶粉料 bonding powder<br />&nbsp;&nbsp;&nbsp; 由无机胶凝材料与各种外加剂在工厂采用预混合干拌技术制成的专门用于配制胶粉聚苯颗粒保温浆料的复合胶凝材料。</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.6 聚苯颗粒expanded polystyrene granule<br />&nbsp;&nbsp;&nbsp; 由聚苯乙烯泡沫塑料经粉碎、混合而制成的具有一定粒度、级配的专门用于配制胶粉聚苯颗粒保温浆料的轻骨料。</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.7 抗裂砂浆 anti-crack mortar<br />&nbsp;&nbsp;&nbsp; 在聚合物乳液中掺加多种外加剂和抗裂物质制得的抗裂剂与普通硅酸盐水泥、中砂按一定比例拌合均匀制成的具有一定柔韧性的砂浆。</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.8 耐碱涂塑玻璃纤维网格布（以下简称耐碱网布） alkali-resistant fiberglass mesh<br />以耐碱玻璃纤维织成的网格布为基布，表面涂覆高分子耐碱涂层制成的网格布。</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.9 高分子乳液弹性底层涂料（以下简称高弹底涂） high polymer latex elastic ground coating由弹性防水乳液加入多种助剂、颜填料配制而成的具有防水和透气效果的封底涂层。 <br />&nbsp;&nbsp;&nbsp; 3.10 抗裂柔性耐水腻子（简称柔性耐水腻子）anti-crack waterproof flexible putty<br />由弹性乳液、助剂和粉料等制成的具有一定柔韧性和耐水性的腻子。&nbsp;</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.11 塑料锚栓 mechanical fixings<br />&nbsp;&nbsp;&nbsp; 由螺钉（塑料钉或具有防腐性能的金属钉）和带圆盘的塑料膨胀套管两部分组成的用于将热镀锌电焊网固定于基层墙体的专用连接件。</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.12 面砖粘结砂浆 adhesive <br />&nbsp;&nbsp;&nbsp; 由聚合物乳液和外加剂制得的面砖专用胶液同强度等级42.5的普通硅酸盐水泥和建筑硅质砂（一级中砂）按一定重量比混合搅拌均匀制成的粘结砂浆。</font></p>
<p><font face="Courier">&nbsp;&nbsp;&nbsp; 3.13 面砖勾缝料 jointing mortar<br />&nbsp;&nbsp;&nbsp; 由高分子材料、水泥、各种填料、助剂复配而成的陶瓷面砖勾缝材料。</font></p>
<p><font face="Courier"><span class="px14"><font id="FontSizeSettings5"></font>&nbsp;</span></font></p>
<p>&nbsp;</p>
<p><font face="Courier">4.分类和标记</font></p>
<p><font face="Courier">4.1 分类<br />胶粉聚苯颗粒外保温系统分为涂料饰面（缩写为C）和面砖饰面（缩写为T）两种类型：<br />&mdash;&mdash;C型胶粉聚苯颗粒外保温系统用于饰面为涂料的胶粉聚苯颗粒外保温系统；<br /></font></p>
<p align="center"><img style="BORDER-RIGHT: #000000 1px solid; BORDER-TOP: #000000 1px solid; BORDER-LEFT: #000000 1px solid; BORDER-BOTTOM: #000000 1px solid" alt="3.3 界面砂浆 interface treating agent" src="http://img.hc360.com/coatings/info/images/200706/p2061101.gif" border="0" /></p>
<p align="center"><span class="px14"><font id="FontSizeSettings5">5 技术要求 </font></span></p>
<div></div>
<div align="left"><br />5.1 胶粉聚苯颗粒外保温系统<br />&nbsp;&nbsp;&nbsp;&nbsp;胶粉聚苯颗粒外保温系统的性能应符合表3的要求。面砖饰面外保温系统抗震性能应满足要求。<font style="FONT-SIZE: 14px"><font style="FONT-SIZE: 14px"></font></font></div>
<p style="FONT-SIZE: 12px" align="center">表3 胶粉聚苯颗粒外保温系统的性能指标 </p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="2">
            <div align="center">试 验 项 目</div>
            </td>
            <td colspan="2">
            <div align="center">性 能 指 标</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">耐候性</div>
            </td>
            <td colspan="2">
            <div align="center">经80次高温(70℃)&mdash;淋水(15℃)循环和20次加热(50℃)&mdash;冷冻(-20℃)循环后不得出现开裂、空鼓或脱落。抗裂防护层与保温层的拉伸粘结强度不应小于0.1MPa，破坏界面应位于保温层。</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center"><br />吸水量，g/m2，浸水1</div>
            </td>
            <td colspan="2">
            <div align="center">h &le; 1000</div>
            </td>
        </tr>
        <tr>
            <td width="25%" rowspan="3">
            <div align="center">抗冲击强度</div>
            </td>
            <td width="22%" rowspan="2">
            <div align="center">C型</div>
            </td>
            <td width="25%">
            <div align="center">普通型（单网）</div>
            </td>
            <td width="28%">
            <div align="center">3.0J冲击合格</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">加强型（双网）</div>
            </td>
            <td>
            <div align="center">10.0J冲击合格</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">T型</div>
            </td>
            <td colspan="2">
            <div align="center">3.0 J冲击合格</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">抗风压值</div>
            </td>
            <td colspan="2">
            <div align="center">不小于工程项目的风荷载设计值</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">耐冻融</div>
            </td>
            <td colspan="2">
            <div align="center">严寒地区30次循环、寒冷及夏热冬冷地区10次循环表面无裂纹、空鼓、起泡、剥离现象</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">水蒸气湿流密度，g/(m2 &middot;h)</div>
            </td>
            <td colspan="2">
            <div align="center">&ge; 0.85</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">不透水性</div>
            </td>
            <td colspan="2">
            <div align="center">试样防护层内侧无水渗透</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">耐磨损，500L砂</div>
            </td>
            <td colspan="2">
            <div align="center">无开裂,龟裂或表面保护层剥落、损伤</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">系统抗拉强度(C型) ,MPa</div>
            </td>
            <td colspan="2">
            <div align="center">&ge;0.1并且破坏部位不得位于各层界面</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">饰面砖粘结强度（T型），MPa(现场抽测)</div>
            </td>
            <td colspan="2">
            <div align="center">&ge;0.4</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">抗震性能（T型）</div>
            </td>
            <td colspan="2">
            <div align="center">设防烈度等级下外保温系统无脱落</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<div align="left">5.2 界面砂浆<br />&nbsp;&nbsp;&nbsp;&nbsp;界面剂及界面砂浆性能应符合表4的要求。</div>
<p align="center">表4 界面剂性能指标 <br /></p>
<p style="FONT-SIZE: 12px" align="left">&nbsp;</p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="2">
            <div align="center">项目</div>
            </td>
            <td width="16%">
            <div align="center">单位</div>
            </td>
            <td width="18%">
            <div align="center">指标</div>
            </td>
        </tr>
        <tr>
            <td width="30%">
            <div align="center">界面剂</div>
            </td>
            <td width="36%">
            <div align="center">不挥发物含量</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&ge;10</div>
            </td>
        </tr>
        <tr>
            <td rowspan="3">
            <div align="center">界面砂浆压剪胶接强度</div>
            </td>
            <td>
            <div align="center">原强度</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.7</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">耐水</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.5</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">耐冻融</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.5</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<div align="left">5.3 胶粉料<br />胶粉料的性能应符合表5的要求。</div>
<p align="center">表5 胶粉料性能指标 <br /></p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td width="34%">
            <div align="center">项 目</div>
            </td>
            <td width="35%">
            <div align="center">单 位</div>
            </td>
            <td width="31%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">初凝时间</div>
            </td>
            <td>
            <div align="center">h</div>
            </td>
            <td>
            <div align="center">&ge;4</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">终凝时间</div>
            </td>
            <td>
            <div align="center">h </div>
            </td>
            <td>
            <div align="center">&le;12</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">安定性（试饼法）</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">合格</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">拉伸粘结强度</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.6</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">浸水拉伸粘结强度</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.4</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<div align="left">5.4 聚苯颗粒轻骨料<br />聚苯颗粒轻骨料的性能应符合表6的要求。</div>
<p align="center">表6 聚苯颗粒轻骨料性能指标<br /></p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td width="34%">
            <div align="left">项 目</div>
            </td>
            <td width="33%">
            <div align="left">单 位</div>
            </td>
            <td width="33%">
            <div align="left">指 标</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="left">堆积密度</div>
            </td>
            <td>
            <div align="left">kg/m3</div>
            </td>
            <td>
            <div align="left">8.0-21.0</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="left">粒度（5mm筛孔筛余）</div>
            </td>
            <td>
            <div align="left">%</div>
            </td>
            <td>
            <div align="left">&le;5</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<font style="FONT-SIZE: 14px">
<p style="FONT-SIZE: 12px" align="left">5.5 胶粉聚苯颗粒保温浆料<br />胶粉聚苯颗粒保温浆料的性能应符合表7的要求。</p>
<p style="FONT-SIZE: 12px" align="center">表7 胶粉聚苯颗粒保温浆料性能指标 </p>
</font>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td width="38%">
            <div align="center">项 目</div>
            </td>
            <td width="33%">
            <div align="center">单 位</div>
            </td>
            <td width="29%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">湿表观密度</div>
            </td>
            <td>
            <div align="center">kg/m3</div>
            </td>
            <td>
            <div align="center">&le;420</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">干表观密度</div>
            </td>
            <td>
            <div align="center">kg/m3</div>
            </td>
            <td>
            <div align="center">&le;250</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">导热系数</div>
            </td>
            <td>
            <div align="center">W/（m&middot;K）</div>
            </td>
            <td>
            <div align="center">&le;0.060</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">蓄热系数</div>
            </td>
            <td>
            <div align="center">W/（m2&middot;K）</div>
            </td>
            <td>
            <div align="center">&ge;0.95</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">抗压强度</div>
            </td>
            <td>
            <div align="center">kPa </div>
            </td>
            <td>
            <div align="center">&ge;250</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">抗拉强度</div>
            </td>
            <td>
            <div align="center">kPa</div>
            </td>
            <td>
            <div align="center">&ge;100</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">压剪粘结强度</div>
            </td>
            <td>
            <div align="center">kPa</div>
            </td>
            <td>
            <div align="center">&ge;50</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">线性收缩率</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&le;0.3</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">软化系数</div>
            </td>
            <td>
            <div align="center">&mdash;&mdash;</div>
            </td>
            <td>
            <div align="center">&ge;0.5</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">难燃性</div>
            </td>
            <td>
            <div align="center">&mdash;&mdash;</div>
            </td>
            <td>
            <div align="center">B1级</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<p style="FONT-SIZE: 12px" align="left"><span class="px14"><font id="FontSizeSettings5">5.6 抗裂砂浆<br />抗裂剂及抗裂砂浆性能应符合表8的要求。 </font></span></p>
<div></div>
<div align="left">&nbsp;</div>
<div align="center">表8 抗裂剂及抗裂砂浆性能指标<br /></div>
<div align="center">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="2">
            <div align="center">项 目</div>
            </td>
            <td width="11%">
            <div align="center">单 位</div>
            </td>
            <td width="59%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td width="6%" rowspan="2">
            <div align="center">抗裂剂</div>
            </td>
            <td width="24%">
            <div align="center">不挥发物含量</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&ge;20</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">贮存稳定性（20℃&plusmn;5℃）</div>
            </td>
            <td>
            <div align="center">--</div>
            </td>
            <td>
            <div align="center">6个月，试样无结块凝聚及发霉现象，且拉伸粘结强度满足抗裂砂浆指标要求。</div>
            </td>
        </tr>
        <tr>
            <td rowspan="4">
            <div align="center">抗裂砂浆</div>
            </td>
            <td>
            <div align="center">可操作时间</div>
            </td>
            <td>
            <div align="center">h</div>
            </td>
            <td>
            <div align="center">&ge;2</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">拉伸粘结强度（常温28d）</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&gt;0.8</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center"><br />浸水拉伸粘结强度（常温28d，浸水7d）</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&gt;0.6</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">压折比</div>
            </td>
            <td>
            <div align="center">-- </div>
            </td>
            <td>
            <div align="center">&le;3.0</div>
            </td>
        </tr>
        <tr>
            <td colspan="4">
            <div align="center">水泥应采用强度等级42.5的普通硅酸盐水泥,并应符合GB 175&mdash;1999的要求；砂应符合JGJ 52&mdash;1992的规定，筛除大于2.5mm颗粒，含泥量少于3%。</div>
            </td>
        </tr>
    </tbody>
</table>
</div>
<p style="FONT-SIZE: 12px" align="left"><br /></p>
<p style="FONT-SIZE: 12px" align="left">5.7 耐碱网布<br />耐碱网布的性能应符合表9的要求。</p>
<p style="FONT-SIZE: 12px" align="center">表9 耐碱网布性能指标</p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="2">
            <div align="center">项 目</div>
            </td>
            <td width="23%">
            <div align="center">单位</div>
            </td>
            <td width="26%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">外观</div>
            </td>
            <td>
            <div align="center">--</div>
            </td>
            <td>
            <div align="center">合格</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">长度、宽度</div>
            </td>
            <td>
            <div align="center">m</div>
            </td>
            <td>
            <div align="center">100、0.9～1.2</div>
            </td>
        </tr>
        <tr>
            <td width="27%" rowspan="2">
            <div align="center">网孔中心距</div>
            </td>
            <td width="24%">
            <div align="center">普通型</div>
            </td>
            <td rowspan="2">
            <div align="center">mm</div>
            </td>
            <td>
            <div align="center">4&times;4</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">加强型</div>
            </td>
            <td>
            <div align="center">6&times;6</div>
            </td>
        </tr>
        <tr>
            <td rowspan="2">
            <div align="center">单位面积质量 </div>
            </td>
            <td>
            <div align="center">普通型</div>
            </td>
            <td rowspan="2">
            <div align="center">g/m2</div>
            </td>
            <td>
            <div align="center">&ge;160</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">加强型</div>
            </td>
            <td>
            <div align="center">&ge;500</div>
            </td>
        </tr>
        <tr>
            <td rowspan="2">
            <div align="center">断裂强力（经纬向）</div>
            </td>
            <td>
            <div align="center">普通型</div>
            </td>
            <td>
            <div align="center">N/50 mm</div>
            </td>
            <td>
            <div align="center">&ge;1250</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">加强型</div>
            </td>
            <td>
            <div align="center">N/50 mm</div>
            </td>
            <td>
            <div align="center">&ge;3000</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">耐碱强力保留率（经纬向）</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&ge;90</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">断裂伸长率</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&le;5</div>
            </td>
        </tr>
        <tr>
            <td rowspan="2">
            <div align="center">涂塑量</div>
            </td>
            <td>
            <div align="center">普通型</div>
            </td>
            <td rowspan="2">
            <div align="center">g/m2</div>
            </td>
            <td rowspan="2">
            <div align="center">&ge;20</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">加强型</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">玻璃成分</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center"><br />符合JC 719的规定，其中ZrO2&ge;14.5，TiO26%&plusmn;0.5</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<p style="FONT-SIZE: 12px" align="left"><br /></p>
<p style="FONT-SIZE: 12px" align="left">5.8 高弹底涂<br />高弹底涂的性能应符合表10的要求。</p>
<p style="FONT-SIZE: 12px" align="center">表10 高弹底涂性能指标</p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="2">
            <div align="center">项 目</div>
            </td>
            <td width="30%">
            <div align="center">单 位</div>
            </td>
            <td width="34%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">容器中状态</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">搅拌后无结块，呈均匀状态</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">施工性</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">刷涂无障碍</div>
            </td>
        </tr>
        <tr>
            <td width="22%" rowspan="2">
            <div align="center">干燥时间</div>
            </td>
            <td width="14%">
            <div align="center">表干时间</div>
            </td>
            <td>
            <div align="center">h </div>
            </td>
            <td>
            <div align="center">&le;4</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">实干时间</div>
            </td>
            <td>
            <div align="center">h</div>
            </td>
            <td>
            <div align="center">&le;8</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">拉伸强度</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;1.0</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">断裂伸长率</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&ge;300</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<p style="FONT-SIZE: 12px" align="left"><span class="px14"><font id="FontSizeSettings5">5.9 柔性耐水腻子<br />柔性耐水腻子的性能应符合表11的要求。 </font></span></p>
<div></div>
<p align="center"><br />表11 柔性耐水腻子性能指标 <br /></p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="3">
            <div align="center">项 目</div>
            </td>
            <td width="22%">
            <div align="center">单 位</div>
            </td>
            <td width="39%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td width="6%" rowspan="10">
            <div align="center">柔性耐水腻子</div>
            </td>
            <td colspan="2">
            <div align="center">施工性</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">刮涂无困难</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">干燥时间（表干）</div>
            </td>
            <td>
            <div align="center">h</div>
            </td>
            <td>
            <div align="center">- </div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">耐水性 48h</div>
            </td>
            <td>
            <div align="center">- </div>
            </td>
            <td>
            <div align="center">无异常</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">耐碱性 24h</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">无异常</div>
            </td>
        </tr>
        <tr>
            <td width="19%" rowspan="2">
            <div align="center">粘结强度 </div>
            </td>
            <td width="14%">
            <div align="center">标准状态</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&gt;0.60</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">浸水后</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&gt;0.40</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">低温贮存稳定性</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">-5℃冷冻4h无变化,刮涂无困难</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">打磨性</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">20-80</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">柔韧性</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">直径50mm,无裂纹</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">透水性（24h）</div>
            </td>
            <td>
            <div align="center">ml </div>
            </td>
            <td>
            <div align="center">&le;3.0</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<div align="left">5.10 外墙外保温饰面涂料<br />外墙外保温饰面涂料必须与胶粉聚苯颗粒外保温系统相容，其性能除应符合国家及行业相关标准外，还应满足表12的抗裂性要求：</div>
<p align="center">表12 外墙外保温饰面涂料抗裂性能指标 <br /></p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="2">
            <div align="center">项 目</div>
            </td>
            <td width="39%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td width="20%" rowspan="3">
            <div align="center">抗裂性</div>
            </td>
            <td width="41%">
            <div align="center">平涂用涂料</div>
            </td>
            <td>
            <div align="center">断裂伸长率&ge;200%</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">连续性复层建筑涂料</div>
            </td>
            <td>
            <div align="center"><br />主涂层的断裂伸长率&ge;100%</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">浮雕类非连续性复层建筑涂料</div>
            </td>
            <td>
            <div align="center">主涂层初期干燥抗裂性满足要求</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<div align="left">5．11 面砖粘结砂浆<br />面砖粘结砂浆性能应符合表13的要求。</div>
<p align="center">表13 面砖粘结砂浆的性能指标<br /></p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="2">
            <div align="center">项 目</div>
            </td>
            <td width="29%">
            <div align="center">单位</div>
            </td>
            <td width="26%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td width="27%" rowspan="2">
            <div align="center">拉伸粘结强度达到0.17MPa时间间隔</div>
            </td>
            <td width="18%">
            <div align="center">晾置时间</div>
            </td>
            <td>
            <div align="center">min</div>
            </td>
            <td>
            <div align="center">不小于10</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">调整时间</div>
            </td>
            <td>
            <div align="center">min</div>
            </td>
            <td>
            <div align="center">大于5</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">拉伸粘结强度</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.60</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">压折比</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">&le;3.0</div>
            </td>
        </tr>
        <tr>
            <td rowspan="3">
            <div align="center">压剪胶接强度</div>
            </td>
            <td>
            <div align="center">原强度</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.6</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">耐温7d</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&ge;0.5</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">耐水7d</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&ge;0.5</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">耐冻融25次</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&ge;0.5</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">线性收缩率</div>
            </td>
            <td>
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&le;0.3</div>
            </td>
        </tr>
        <tr>
            <td colspan="4">
            <div align="center">水泥应采用强度等级42.5的普通硅酸盐水泥,并应符合GB 175&mdash;1999的要求；砂应符合JGJ 52&mdash;1992的规定，筛除大于2.5mm颗粒，含泥量少于3%。</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<p style="FONT-SIZE: 12px" align="left"><span class="px14"><font id="FontSizeSettings5">5．12 面砖勾缝料<br />面砖勾缝料的性能应符合表14的要求。 </font></span></p>
<div></div>
<p align="center">表14 面砖勾缝料性能指标<br /></p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="2">
            <div align="center">项 目</div>
            </td>
            <td width="15%">
            <div align="center">单位 </div>
            </td>
            <td width="48%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">外 观</div>
            </td>
            <td>
            <div align="center">- </div>
            </td>
            <td>
            <div align="center">均匀一致</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">凝结时间</div>
            </td>
            <td>
            <div align="center">h</div>
            </td>
            <td>
            <div align="center">大于2小时，小于24小时</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">颜 色</div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">与标准样一致</div>
            </td>
        </tr>
        <tr>
            <td width="16%" rowspan="2">
            <div align="center">拉伸胶接强度 </div>
            </td>
            <td width="21%">
            <div align="center">常温常态14d</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.60</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">耐水（常温常态14d，浸水48h，放置24h）</div>
            </td>
            <td>
            <div align="center">MPa</div>
            </td>
            <td>
            <div align="center">&ge;0.50</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">压折比（抗压强度/抗折强度） </div>
            </td>
            <td>
            <div align="center">-</div>
            </td>
            <td>
            <div align="center">&le;3</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">透水性（24h）</div>
            </td>
            <td>
            <div align="center">ml </div>
            </td>
            <td>
            <div align="center">&le;3.0</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<div align="left">5.13 塑料锚栓<br />&nbsp;&nbsp;&nbsp; 塑料锚栓通常由螺钉和带圆盘的塑料膨胀套管两部分组成，金属螺钉应采用不锈钢或经过表面防锈蚀处理的金属制成，塑料钉和带圆盘的塑料膨胀套管应采用聚酰胺（polyamide 6、polyamide 6.6）、聚乙烯 (polyethylene)或聚丙烯 (polypropylene)制成，制作塑料钉和塑料套管的材料不得使用回收的再生材料。塑料锚栓有效锚固深度不小于25 mm，塑料圆盘直径不小于50 mm，单个塑料锚栓抗拉承载力标准值（C25混凝土基层）不小于0.80 kN。</div>
<div align="left"><br />5.14 热镀锌电焊网</div>
<div align="left"><br />&nbsp;&nbsp;&nbsp; 热镀锌电焊网（俗称四角网）应符合《镀锌电焊网》QB/T3897&mdash;1999标准并满足表15的要求。</div>
<div align="center"><br />表15 热镀锌电焊网性能指标</div>
<p style="FONT-SIZE: 12px" align="left"><br /></p>
<p style="FONT-SIZE: 12px" align="left">
<table cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td width="35%">
            <div align="center">项 目</div>
            </td>
            <td width="23%">
            <div align="center">单位</div>
            </td>
            <td width="42%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">工艺</div>
            </td>
            <td>
            <div align="center">--</div>
            </td>
            <td>
            <div align="center">热镀锌电焊网</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">丝径</div>
            </td>
            <td>
            <div align="center">mm</div>
            </td>
            <td>
            <div align="center">0.9</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">网孔大小</div>
            </td>
            <td>
            <div align="center">mm</div>
            </td>
            <td>
            <div align="center">12.7&times;12.7</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">焊点抗拉力</div>
            </td>
            <td>
            <div align="center">N</div>
            </td>
            <td>
            <div align="center">&gt;65</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">镀锌层重量</div>
            </td>
            <td>
            <div align="center">g/m2</div>
            </td>
            <td>
            <div align="center">&ge;122</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<div align="left">5.15 饰面砖<br />外保温饰面砖应采用粘贴面带有燕尾槽的产品并不得带有脱模剂。其性能应符合下列现行标准的要求：《陶瓷砖和卫生陶瓷分类及术语》GB/T 9195；《干压陶瓷砖》GB/T 4100.1、GB/T 4100.2、 GB/T 4100.3、 GB/T 4100.4；《陶瓷劈离砖》JC/T 457；《玻璃马赛克》GB/T 7697。并应同时满足表16性能指标的要求。</div>
<p align="center">表16 饰面砖性能指标<br /></p>
<p style="FONT-SIZE: 12px" align="left">
<table cellspacing="1" cellpadding="0" width="100%" border="1">
    <tbody>
        <tr>
            <td colspan="3">
            <div align="center">项 目</div>
            </td>
            <td width="25%">
            <div align="center">单位</div>
            </td>
            <td width="27%">
            <div align="center">指 标</div>
            </td>
        </tr>
        <tr>
            <td width="16%" rowspan="4">
            <div align="center">尺寸</div>
            </td>
            <td width="18%" rowspan="2">
            <div align="center">6m以下墙面</div>
            </td>
            <td width="14%">
            <div align="center">表面面积</div>
            </td>
            <td>
            <div align="center">cm2</div>
            </td>
            <td>
            <div align="center">&le;410</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">厚度</div>
            </td>
            <td>
            <div align="center">cm</div>
            </td>
            <td>
            <div align="center">&le;1.0</div>
            </td>
        </tr>
        <tr>
            <td rowspan="2">
            <div align="center">6m及以上墙面</div>
            </td>
            <td>
            <div align="center">表面面积</div>
            </td>
            <td>
            <div align="center">cm2</div>
            </td>
            <td>
            <div align="center">&le;190</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">厚度</div>
            </td>
            <td>
            <div align="center">cm</div>
            </td>
            <td>
            <div align="center">&le;0.75</div>
            </td>
        </tr>
        <tr>
            <td colspan="3">
            <div align="center">单位面积质量</div>
            </td>
            <td>
            <div align="center">kg/m2</div>
            </td>
            <td>
            <div align="center">&le;20</div>
            </td>
        </tr>
        <tr>
            <td rowspan="2">
            <div align="center">吸水率</div>
            </td>
            <td colspan="2">
            <div align="center">Ⅰ、Ⅵ、Ⅶ气候区</div>
            </td>
            <td rowspan="2">
            <div align="center">%</div>
            </td>
            <td>
            <div align="center">&le;3</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">Ⅱ、Ⅲ、Ⅳ、Ⅴ气候区</div>
            </td>
            <td>
            <div align="center">&le;6</div>
            </td>
        </tr>
        <tr>
            <td>
            <div align="center">抗冻性</div>
            </td>
            <td colspan="2">
            <div align="center">Ⅰ、Ⅵ、Ⅶ气候区</div>
            </td>
            <td>
            <div align="center"><br />--</div>
            </td>
            <td>
            <div align="center">50次冻融循环无破坏</div>
            </td>
        </tr>
        <tr>
            <td rowspan="2">
            <div align="left">&nbsp;</div>
            </td>
            <td colspan="2">
            <div align="center">Ⅱ气候区</div>
            </td>
            <td rowspan="2">
            <div align="left">&nbsp;</div>
            </td>
            <td>
            <div align="center">40次冻融循环无破坏</div>
            </td>
        </tr>
        <tr>
            <td colspan="2">
            <div align="center">Ⅲ、Ⅳ、Ⅴ气候区</div>
            </td>
            <td>
            <div align="center">10次冻融循环无破坏</div>
            </td>
        </tr>
        <tr>
            <td colspan="5">
            <div align="center">注：气候区划分级按GB 50178&mdash;1993 中一级区划的Ⅰ～Ⅶ区执行。</div>
            </td>
        </tr>
    </tbody>
</table>
</p>
<div align="left">5.16 附件<br />在胶粉聚苯颗粒外保温系统中所采用的附件，包括密封膏、密封条、金属护角、盖口条等应分别符合相应的产品标准的要求。 </div>
<div align="left">
<p>6 试验方法<br />&nbsp;&nbsp;&nbsp;&nbsp;凡国标或行标中已有规定的均按有关规定进行。标准试验环境为空气温度（23&plusmn;2）℃，相对湿度（50&plusmn;10）%。在非标准试验环境下试验时，应记录温度和相对湿度。<br />6.1 胶粉聚苯颗粒外保温系统<br />6.1.1 耐候性<br />按附录A的规定进行。<br />6.1.2 吸水量<br />按附录B的规定进行。<br />6.1.3 抗冲击强度<br />6.1.3.1 试样<br />&nbsp;&nbsp;&nbsp;&nbsp;a） C型单网普通试样：<br />数量：2件，每件分别用于3J级和10J级冲击试验；<br />尺寸： 1200mm&times;600mm，保温层厚度50mm<br />制作：50 mm胶粉聚苯颗粒保温层（7d）+4mm抗裂砂浆（压入耐碱网布，网布不得有搭接缝）（5d）+高弹底涂（24h）+柔性耐水腻子，在试验室环境下养护56d后，涂刷饰面涂料，涂料实干后，待用。<br />&nbsp;&nbsp;&nbsp;&nbsp;b） C型双网加强试样：<br />数量：2件，每件分别用于3J级和10J级冲击试验；<br />尺寸： 1200mm&times;600mm，保温层厚度50mm<br />制作：50 mm胶粉聚苯颗粒保温层（5d）+4mm抗裂砂浆（先压入一层加强型耐碱网布，再压入一层耐碱网布，网布不得有搭接缝）（5d）+高弹底涂（24h）+柔性耐水腻子，在试验室环境下养护56d后，涂刷饰面涂料，涂料实干后，待用。<br />&nbsp;&nbsp;&nbsp;&nbsp;c）T型试样：<br />数量：2件，每件分别用于3J级和10J级冲击试验；<br />尺寸： 1200mm&times;600mm，保温层厚度50mm<br />制作：50 mm胶粉聚苯颗粒保温层（5d）+4mm抗裂砂浆（压入热镀锌电焊网）（24h）+4mm抗裂砂浆（5d）+粘贴面砖（2d）+勾缝，在试验室环境下养护56d。<br />6.1.3.2 试验过程<br />&nbsp;&nbsp;&nbsp;&nbsp;a） 将试样抗裂防护层向上平放于光滑的刚性底板上。<br />&nbsp;&nbsp;&nbsp;&nbsp;b） 试验分为3J和10J两级，每级试验冲击10个点。3J级冲击试验使用质量为500g的钢球，在距离试样上表面0.61m高度自由降落冲击试样。10J级冲击试验使用质量为1000g的钢球，在距离试样上表面1.02m高度自由降落冲击试样。冲击点应离开试样边缘至少100mm，冲击点间距不得小于100mm。以冲击点及其周围开裂作为破坏的判定标准。<br />6.1.3.3 试验结果<br />10J级试验10个冲击点中破坏点不超过4个时，判定为10J冲击合格。10J级试验10个冲击点中破坏点超过4个，3J级试验10个冲击点中破坏点不超过4个时，判定为3J冲击合格。<br />6.1.4 抗风压<br />按附录C的规定进行。<br />6.1.5 耐冻融<br />6.1.5.1 试验仪器<br />&nbsp;&nbsp;&nbsp;&nbsp;a） 低温冷冻箱 最低温度-30℃&plusmn;3℃<br />&nbsp;&nbsp;&nbsp;&nbsp;b） 密封材料：松香、石蜡<br />6.1.5.2 试样：<br />&nbsp;&nbsp;&nbsp;&nbsp;a） C型试样：<br />数量：3 个，尺寸：500 mm &times; 500 mm的试件；<br />制作： 50 mm胶粉聚苯颗粒保温层（5d）+4mm抗裂砂浆（压入标准耐碱网布）（5d）+高弹底涂，在试验室环境下养护56d。除试件涂料面外将其它5面用融化的松香、石蜡（1：1）密封。<br />&nbsp;&nbsp;&nbsp;&nbsp;b） T型试样：<br />数量：3 个，尺寸：500 mm &times; 500 mm的试件；<br />制作： 见6.1.3.1中c）。除面砖这一面外将其它5面用融化的松香、石蜡（1：1）密封。<br />6.1.5.3 试验过程<br />&nbsp;&nbsp;&nbsp;&nbsp;冻融循环30次，每次24h<br />&nbsp;&nbsp;&nbsp;&nbsp;a） 在20&plusmn;2℃自来水中浸泡8h。试样浸入水中时，应使抗裂防护层朝下，使抗裂防护层浸入水中，并排除试样表面气泡。<br />&nbsp;&nbsp;&nbsp;&nbsp;b） 在-20&plusmn;2℃冰箱中冷冻16h。<br />试验期间如需中断试验，试样应置于冰箱中在-20&plusmn;2℃下存放。<br />6.1.5.4 试验结果<br />&nbsp;&nbsp;&nbsp;&nbsp;每3次循环后观察试样是否出现裂纹、空鼓、起泡、剥离等情况并做记录。经10次、20次、30次冻融循环试验后观察，试样无裂纹、空鼓、起泡、剥离者为10次、20次、30次冻融循环合格。<br />6.1.6 水蒸气湿流密度<br />&nbsp;&nbsp;&nbsp;&nbsp;按GB/T 17146&mdash;1997的规定进行。<br />6.1.7 不透水性<br />&nbsp;&nbsp;&nbsp;&nbsp;按附录D的规定进行。<br />6.1.8 耐磨损<br />&nbsp;&nbsp;&nbsp;&nbsp;按附录E的规定进行。<br />6.1.9 系统抗拉强度<br />&nbsp;&nbsp;&nbsp;&nbsp;按附录F的规定进行。<br />6.1.10 饰面砖粘结强度<br />&nbsp;&nbsp;&nbsp;&nbsp;系统完成56天后，按JGJ 110&mdash;1997的规定进行饰面砖粘结强度拉拔试验。断缝应从饰面砖表面切割至抗裂防护层表面（不应露出热镀锌电焊网），深度应一致。<br />6.1.11 抗震性能<br />&nbsp;&nbsp;&nbsp;&nbsp;按附录G的规定进行。<br />6.2 界面剂及界面砂浆<br />6.2.1 界面剂不挥发物含量<br />&nbsp;&nbsp;&nbsp;&nbsp;按GB/T 2793&mdash;1995的规定进行。<br />6.2.2 界面砂浆压剪胶接强度 <br />&nbsp;&nbsp;&nbsp;&nbsp;按JC/T 547&mdash;1994 中6.3.4条规定进行测定。原强度：在试验室环境条件下养护14天；耐水：在试验条件空气中养护14天，然后在试验条件水中浸泡７天，取出擦干表面水份，进行测定；耐冻融：在试验条件空气中养护14天，然后按GBJ 82-1985抗冻性能试验循环10次。<br />6.3 胶粉料<br />6.3.1 初凝时间、终凝时间和安定性<br />6.3.1.1 按GB/T 1346－2001中7的规定测定标准稠度用水量。<br />6.3.1.2 按GB/T 1346－2001中8的规定测定初凝时间、终凝时间。配料时在胶砂搅拌机中搅拌3分钟。<br />6.3.1.3 按GB/T 1346－2001中11的规定测定安定性。配料时在胶砂搅拌机中搅拌3分钟。<br />6.3.2 拉伸粘结强度、浸水拉伸粘结强度<br />&nbsp;&nbsp;&nbsp;&nbsp;按JG/T 24&mdash;2000中6.14的规定进行。<br />6.3.2.1 试样<br />&nbsp;&nbsp;&nbsp;&nbsp;制作：在10个 70 mm &times; 70 mm &times; 20 mm水泥砂浆试块上，在标准稠度用水量条件下按JG/T 24&mdash;2000中6.14.2.1的规定成型试块.<br />养护：用湿布覆盖后再用聚乙烯薄膜覆盖，在试验室温度条件下养护2天。去掉覆盖物后装入塑料袋中在试验室温度条件下继续养护25天，用双组份环氧树脂或其它高强度粘结剂粘结钢质上夹具。放置24h。<br />6.3.2.2 试验过程<br />&nbsp;&nbsp;&nbsp;&nbsp;其中5个试件按JG/T 24&mdash;2000中6.14.2.2的规定测抗拉强度即为拉伸粘结强度。<br />另5个试件按JG/T 24&mdash;2000中6.14.3.2的规定测浸水7d的抗拉强度即为浸水拉伸粘结强度<br />6.4 聚苯颗粒<br />6.4.1 堆积密度<br />&nbsp;&nbsp;&nbsp;&nbsp;按JC 209－1992中6.1的规定进行。<br />6.4.2 轻骨料粒度<br />&nbsp;&nbsp;&nbsp;&nbsp;按JC 209－1992中6.3的规定进行。烘干温度为50℃&plusmn;2℃，筛孔尺寸为5mm。</p>
<p>6.5 胶粉聚苯颗粒保温浆料<br />标准胶粉聚苯颗粒保温浆料（简称标准浆料）制备：按厂家产品说明书中规定的比例和方法，在胶砂搅拌机中加入水和胶粉料，搅拌均匀后加入聚苯颗粒继续搅拌至均匀。<br />6.5.1 湿表观密度<br />6.5.1.1 仪器设备<br />&nbsp;&nbsp;&nbsp;&nbsp;a）标准量筒：容积为0.001m3，要求内壁光洁，并具有足够的刚度，标准量筒应定期进行校核。<br />&nbsp;&nbsp;&nbsp;&nbsp;b）天平：精度为0.01g。<br />&nbsp;&nbsp;&nbsp;&nbsp;c）油灰刀，抹子；<br />&nbsp;&nbsp;&nbsp;&nbsp;d）捣棒：直径10mm，长350mm的钢棒，端部应磨圆；<br />6.5.1.2 试验步骤<br />&nbsp;&nbsp;&nbsp;&nbsp;将称量过的标准量筒，用油灰刀将标准浆料填满量筒，使稍有富余，用捣棒均匀插捣25次（插捣过程中如浆料沉落到低于筒口，则应随时填加浆料），然后用抹子抹平，将量筒外壁擦净，称量浆料与量筒的总重，精确至0.001 kg。<br />6.5.1.3 结果计算<br />&nbsp;&nbsp;&nbsp;&nbsp;浆料湿密度按式（1）计算：<br />&rho;=(m1-m0)/v &hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;（1）<br />式中：<br />&rho;&mdash;浆料湿密度，kg/m3；<br />m0&mdash;容量筒质量， kg；<br />m1&mdash;浆料加容量筒的质量，kg；<br />v&mdash;容量筒的体积，m3。<br />试验结果取三次试验结果算术平均值，保留三位有效数字。<br />6.5.2 干表观密度<br />6.5.2.1 仪器设备<br />&nbsp;&nbsp;&nbsp;&nbsp;a）烘箱：灵敏度&plusmn;2℃；<br />&nbsp;&nbsp;&nbsp;&nbsp;b）天平：精度为0.01g。<br />&nbsp;&nbsp;&nbsp;&nbsp;c）干燥器：直径大于300mm；<br />&nbsp;&nbsp;&nbsp;&nbsp;d）游标卡尺：0～125mm；精度0.02mm；<br />&nbsp;&nbsp;&nbsp;&nbsp;e）钢板尺：500mm，精度：1mm；<br />&nbsp;&nbsp;&nbsp;&nbsp;f）油灰刀，抹子；<br />&nbsp;&nbsp;&nbsp;&nbsp;g）组合式无底金属试模：300mm&times;300mm&times;30mm；<br />&nbsp;&nbsp;&nbsp;&nbsp;h）玻璃板：400mm&times;400mm&times;(3～5)mm；<br />6.5.2.2 试件制备<br />&nbsp;&nbsp;&nbsp;&nbsp;成型方法：将三个空腔尺寸为300mm&times;300mm&times;30mm的金属试模分别放在玻璃板上，用脱模剂涂刷试模内壁及玻璃板，用油灰刀将标准浆料逐层加满并略高出试模，为防止浆料留下孔隙，用油灰刀沿模壁插数次，然后用抹子抹平，制成三个试件。<br />养护方法：试件成型后用湿布覆盖再用聚乙烯薄膜覆盖，在试验室温度条件下养护7天后拆模，拆模后干养护7天，然后将试件放入70℃&plusmn;2℃的烘箱中，烘干至恒重，取出放入干燥器中冷却至室温备用。<br />6.5.2.3 试验步骤<br />&nbsp;&nbsp;&nbsp;&nbsp;取制备好的三块试件分别磨平并称量质量，精确至1g。按顺序用钢板尺在试件两端距边缘20mm处和中间位置分别测量其长度和宽度，精确至1mm，取三个测量数据的平均值。<br />&nbsp;&nbsp;&nbsp;&nbsp;用游标卡尺在试件任何一边的两端距边缘20mm和中间处分别测量厚度，在相对的另一边重复以上测量，精确至0.1mm，要求试件厚度差小于2%，否则重新打磨试件，直至达到要求。最后取6个测量数据的平均值。<br />由以上测量数据求得每个试件的质量与体积。<br />6.5.2.4 结果计算<br />&nbsp;&nbsp;&nbsp;&nbsp;干表观密度按（2）计算：<br />&rho;=m/v &hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;（2）<br />式中<br />&rho;&mdash;干密度，kg/m3；<br />m&mdash;试件质量，kg;<br />v&mdash;试件体积，m3。 <br />&nbsp;&nbsp;&nbsp;&nbsp;试验结果取三个试件试验结果的算术平均值，保留三位有效数字。 <br />6.5.3 导热系数<br />&nbsp;&nbsp;&nbsp;&nbsp;测试干表观密度后的试件，按GB/T 10294－1988的规定测试导热系数。<br />6.5.4 蓄热系数<br />&nbsp;&nbsp;&nbsp;&nbsp;按JGJ 51&mdash;2002中7.5的规定进行。<br />6.5.5 抗压强度<br />6.5.5.1 仪器设备<br />&nbsp;&nbsp;&nbsp;&nbsp;a）钢质有底试模100mm&times;100mm&times;100mm，应具有足够的刚度并拆装方便。试模的内表面不平整度应为每100mm不超过0.05mm，组装后各相邻面的不垂直度小于0.5度；<br />&nbsp;&nbsp;&nbsp;&nbsp;b）捣棒：直径10mm，长350mm的钢棒，端部应磨圆；<br />&nbsp;&nbsp;&nbsp;&nbsp;c）压力试验机：精度（示值的相对误差）小于&plusmn;2%，量程应选择在材料的预期破坏荷载相当于仪器刻度的20%～80%之间；试验机的上、下压板的尺寸应大于试件的承压面，其不平整度应为每100mm 不超过0.02mm。<br />6.5.5.2 试件制备<br />&nbsp;&nbsp;&nbsp;&nbsp;成型方法：将金属模具内壁涂刷脱模剂，向试模内注满标准浆料并略高于试模的上表面，用捣棒均匀由外向里按螺旋方向插捣25次，为防止浆料留下孔隙，用油灰刀沿模壁插数次，然后将高出的浆料沿试模顶面削去用抹子抹平。须按相同的方法同时成型10块试件，其中5个测抗压强度，另5个用来测软化系数。<br />养护方法：试块成型后用湿布覆盖再用聚乙烯薄膜覆盖，在试验室温度条件下养护2天后去掉覆盖物，对试件进行编号并拆模。然后将试件放入塑料袋中，封闭袋口，在标准试验条件下继续养护26天。第28天将试件取出放入70℃&plusmn;2℃的烘箱中烘至恒重，恒重后的试件从烘箱中取出放入干燥器中备用。</p>
<p>6.5.5.3 试验步骤<br />&nbsp;&nbsp;&nbsp;&nbsp;抗压强度：从干燥器中取出的试件应尽快进行试验，以免试件内部的温湿度发生显著的变化。取出其中的5块测量试件的承压面积，长宽测量精确到1mm，并据此计算试件的受压面积。将试件安放在压力试验机的下压板上，试件的承压面应与成型时的顶面垂直，试件中心应与试验机下压板中心对准。开动试验机，当上压板与试件接近时，调整球座，使接触面均衡受压。承压试验应连续而均匀地加荷，加荷速度应为每秒钟0.5～1.5KN，直至试件破坏，然后记录破坏荷载N0 。<br />6.5.5.4 结果计算 <br />&nbsp;&nbsp;&nbsp;&nbsp;抗压强度按式（3）计算：<br />f0=N0/A &hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;(3)<br />式中f0&mdash;抗压强度，kPa;<br />N0&mdash;破坏压力，kN；<br />A&mdash;试件的承压面积，mm2。<br />&nbsp;&nbsp;&nbsp;&nbsp;试验结果以5个试件测值的算术平均值作为该组试件的抗压强度，保留三位有效数字。当五个试件的最大值或最小值与平均值的差超过20%时，以中间三个试件的平均值作为该组试件的抗压强度值。<br />6.5.6 软化系数<br />&nbsp;&nbsp;&nbsp;&nbsp;取6.5.5.2余下的5块试件，将其浸入到20&plusmn;5℃的水中（用铁篦子将试件压入水面下20mm处），48h后取出，在试验室条件下放置24小时，然后按照6.5.5.3和6.5.5.4所述方法测定其浸水后的抗压强度f1。<br />软化系数按式（4）进行计算：<br />&psi;= f1/ f0 (4) <br />式中：<br />&psi;&mdash;软化系数；<br />f0&mdash;绝干状态下的抗压强度，kPa；<br />f1&mdash;浸水后的抗压强度，kPa；<br />6.5.7 抗拉强度<br />6.5.7.1 仪器设备<br />&nbsp;&nbsp;&nbsp;&nbsp;a）试模尺寸100mm&times;100mm&times;50mm，其他要求同6.5.5.1条款的（1）；<br />&nbsp;&nbsp;&nbsp;&nbsp;b）拉力试验机：精度（示值的相对误差）小于&plusmn;2%，破坏荷载相当于仪器刻度的15%～85%的拉力试验机。<br />&nbsp;&nbsp;&nbsp;&nbsp;c）尺寸为100mm&times;100mm&times;5mm的金属试验板，应具有足够的刚度， 100mm&times;100mm平面的中心设有一个能够与拉力试验机连接的接头，另一平面的表面不平整度为100mm小于0.05mm；<br />6.5.7.2 试件制备<br />&nbsp;&nbsp;&nbsp;&nbsp;试件尺寸为100mm&times;100mm&times;50mm，制作5个，方法同 6.5.5.2。<br />6.5.7.3 试验步骤：<br />&nbsp;&nbsp;&nbsp;&nbsp;a）从干燥器中取出试块，用砂纸磨平测试面，厚度差小于2%，用双组份环氧胶将试块上下表面分别与尺寸为100mm&prime;100mm&times;5mm的试验板粘结。放入干燥器中24h。<br />&nbsp;&nbsp;&nbsp;&nbsp;b）通过万向接头将试块安装于拉力试验机上，以5mm/min的拉伸速度拉伸至试件破坏，记录破坏时的拉力及破坏部位。破坏部位在试验板粘结界面时试验数据无效。<br />6.5.7.4 结果计算<br />&nbsp;&nbsp;&nbsp;&nbsp;抗拉强度按式（5）进行计算。<br />st = Pt/ A &hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;(5)<br />式中：<br />st&mdash;抗拉强度，kPa；<br />Pt&mdash;破坏荷载，kN；<br />A&mdash;试样面积，mm2。<br />&nbsp;&nbsp;&nbsp;&nbsp;试验结果按6.5.5.5处理。<br />6.5.8 压剪粘结强度<br />6.5.8.1 仪器设备<br />&nbsp;&nbsp;&nbsp;&nbsp;a）压力试验机：同6.5.5.1条款中（1）的要求；<br />&nbsp;&nbsp;&nbsp;&nbsp;b）水泥砂浆块 ：110mm&times;110mm&times;10mm 10块 <br />6.5.8.2 试件制备<br />&nbsp;&nbsp;&nbsp;&nbsp;将标准浆料涂抹于相对的两个规格为110mm&times;110mm&times;10mm水泥砂浆块间，两水泥砂浆块相对并错开10mm，得到的浆料面积为100mm&times;110mm，厚度10mm。成型5个试件，用湿布覆盖再用聚乙烯薄膜覆盖，在试验室温度条件下养护2天。去掉覆盖物后将试块装入塑料袋中在试验室标准条件下养护26天，将试件取出放入70℃&plusmn;2℃的烘箱中烘至恒重，然后取出放在干燥器中冷却待用。<br />6.5.8.3 试验步骤<br />&nbsp;&nbsp;&nbsp;&nbsp;将试件从干燥器中取出尽快进行压力测试。将试件置于试验机加荷台中心，以5mm/min的速度均匀加荷至试件破坏，记录破坏时的荷载值。<br />6.5.8.4 结果计算<br />&nbsp;&nbsp;&nbsp;&nbsp;压剪粘结强度按式（6）计算：<br />Rn=P/A &hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;（6）<br />式中<br />Rn&mdash;压剪粘结强度，kPa；<br />P&mdash;破坏荷载，kN；<br />A&mdash; 粘结面积，mm2。<br />&nbsp;&nbsp;&nbsp;&nbsp;试验结果按6.5.5.5处理。<br />6.5.9 线性收缩率<br />&nbsp;&nbsp;&nbsp;&nbsp;按JGJ70-90中第十章进行。<br />6.5.9.1试验仪器<br />&nbsp;&nbsp;&nbsp;&nbsp;JGJ70-90中第10.0.2条的规定。<br />6.5.9.2试验步骤 <br />&nbsp;&nbsp;&nbsp;&nbsp;（1） 将收缩头固定在试模两端的孔洞中，使收缩头露出试件端面8&plusmn;1mm；<br />&nbsp;&nbsp;&nbsp;&nbsp;（2） 将试模内壁涂刷脱模剂，向试模内注满标准浆料并略高于试模的上表面，用捣棒均匀插捣25次，为防止浆料留下孔隙，用油灰刀沿模壁插数次，然后将高出的浆料沿试模顶面削去抹平。试块成型后用湿布覆盖再用聚乙烯薄膜覆盖，在试验室温度条件下养护7天后去掉覆盖物，对试件进行编号、拆模并标明测试方向。然后用标准杆调整收缩仪的百分表的零点，按标明的测试方向立即测定试件的长度，即为初始长度；<br />&nbsp;&nbsp;&nbsp;&nbsp;（3） 测定初始长度后，将试件放在标准试验条件下继续养护21天。第28天测定试件的长度，即为干燥后长度。<br />6.5.9.3 结果计算：<br />&nbsp;&nbsp;&nbsp;&nbsp;收缩率按式（7）计算：<br />&epsilon;=（L0-L1）/(L-Ld) &hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;（7）<br />式中：<br />&epsilon;&mdash;自然干燥收缩率<br />L0&mdash;试件的初始长度<br />L1&mdash;试件干燥后的长度<br />L&mdash;试件的长度160mm<br />Ld&mdash;两个收缩头埋入砂浆中长度之和，即20&plusmn;2mm</p>
<p>6.5.9.4 试验结果按三个试件测定值的算术平均值来确定，如个别值与平均值偏差大于20%，应剔除，但一组至少有两个数据计算平均值；实验结果取两位有效数字，精确到10&times;10-6。<br />6.5.10 难燃性<br />&nbsp;&nbsp;&nbsp;&nbsp;按GB/T 8625－1988的规定进行。<br />6.6 抗裂剂及抗裂砂浆<br />&nbsp;&nbsp;&nbsp;&nbsp;标准抗裂砂浆的制备：按厂家产品说明书中规定的比例和方法，在胶砂搅拌机中加入抗裂剂和标准砂，搅拌均匀后加入强度等级为42.5的普通硅酸盐水泥继续搅拌至均匀即为标准抗裂砂浆。抗裂砂浆的性能均应采用标准抗裂砂浆进行测试。<br />6.6.1 抗裂剂不挥发物含量<br />&nbsp;&nbsp;&nbsp;&nbsp;按GB/T 2793&mdash;1995的规定进行。试验温度105℃&plusmn;2℃，试验时间180min&plusmn;5min，取样量2.0g。<br />6.6.2 抗裂剂贮存稳定性<br />&nbsp;&nbsp;&nbsp;&nbsp;从刚生产的抗裂剂中取样，装满3个容量为500mL有盖容器。在20℃&plusmn;5℃条件下放置6个月，观察试样有无结块、凝聚及发霉现象，并按6.6.5的规定测抗裂砂浆的拉伸粘结强度，粘结强度不低于表8拉伸粘结强度原强度的要求。<br />6.6.3 抗裂砂浆可操作时间<br />&nbsp;&nbsp;&nbsp;&nbsp;标准抗裂砂浆配制好后，在试验环境中按制造商提供的可操作时间（没有规定时按2h）放置，然后按6.6.4中拉伸粘结强度测试的规定进行，试验结果以5个试验数据的算术平均值表示，平均粘结强度不低于表8拉伸粘结强度原强度的要求。<br />6.6.4 抗裂砂浆拉伸粘结强度、浸水拉伸粘结强度<br />&nbsp;&nbsp;&nbsp;&nbsp;按JG/T 24&mdash;2000中6.14的规定进行。<br />6.6.4.1 试样<br />&nbsp;&nbsp;&nbsp;&nbsp;在10个 70 mm &times; 70 mm &times; 20 mm水泥砂浆试块上，用标准抗裂砂浆按JG/T 24&mdash;2000中6.14.2.1的规定成型试块，试块装入塑料袋中在试验室温度条件下养护14天，取出，试验室标准条件下继续养护13天。用双组份环氧树脂或其它高强度粘结剂粘结钢质上夹具，放置24h。<br />6.6.4.2 试验过程<br />&nbsp;&nbsp;&nbsp;&nbsp;其中5个试件按JG/T 24&mdash;2000中6.14.2.2的规定测抗拉强度即为拉伸粘结强度。<br />另5个试件按JG/T 24&mdash;2000中6.14.3.2的规定测浸水7d的抗拉强度即为浸水拉伸粘结强度<br />6.6.6 抗裂砂浆压折比<br />&nbsp;&nbsp;&nbsp;&nbsp;a） 抗压强度、抗折强度测定按GB/T 17671&mdash;1999的规定进行。养护条件：采用标准抗裂砂浆成型，用湿布覆盖再用聚乙烯薄膜覆盖，在试验室标准条件下养护4天后脱模，去掉覆盖物后将试块装入塑料袋中在试验室温度条件下养护10天，将试件取出继续在试验室标准条件下养护14天。<br />&nbsp;&nbsp;&nbsp;&nbsp;b） 压折比的计算： <br />压折比按式（7）计算<br />T =Rc/Rf &hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;&hellip;(7)<br />式中：<br />T &mdash;&mdash;压折比<br />Rc &mdash;&mdash;抗压强度，N/mm2<br />Rf&mdash;&mdash;抗折强度, N/mm2</p>
<p>6.7 耐碱网布<br />6.7.1 外观<br />&nbsp;&nbsp;&nbsp;&nbsp;按JC/T 841－1999中5.2的规定进行。<br />6.7.2 长度及宽度<br />&nbsp;&nbsp;&nbsp;&nbsp;按GB/T 7689.3&mdash;2001的规定进行。<br />6.7.3 网孔中心距<br />&nbsp;&nbsp;&nbsp;&nbsp;用直尺测量连续10个孔的平均值。<br />6.7.4 单位面积质量<br />&nbsp;&nbsp;&nbsp;&nbsp; 按GB/T 9914.3&mdash;2001的规定进行。<br />6.7.5 断裂强力<br />&nbsp;&nbsp;&nbsp;&nbsp;按GB/T 7689.5&mdash;2001中类型Ⅰ的规定测经向和纬向的断裂强力。<br />6.7.6 耐